Allgemein
Property | Value | Testing Standard |
---|---|---|
Dichte | 1.01 - 1.07 g/cm³ Show Supplier Material materials with Dichte of 1.01 - 1.07 g/cm³ | ASTM D792 |
Mechanisch
Property | Value | Testing Standard | Comment |
---|---|---|---|
Dehnung | 502.9 % Show Supplier Material materials with Dehnung of 502.9 % | ASTM D412 | 500 mm/min |
Härte, Shore A | 62 - 68 [-] Show Supplier Material materials with Härte, Shore A of 62 - 68 [-] | ASTM D2240 | |
Modul bei 100 % Dehnung | 0.00181 GPa Show Supplier Material materials with Modul bei 100 % Dehnung of 0.00181 GPa | ASTM D412 | 500 mm/min |
Modul bei 300 % Dehnung | 0.00261 GPa Show Supplier Material materials with Modul bei 300 % Dehnung of 0.00261 GPa | ASTM D412 | 500 mm/min |
Reißfestigkeit | 20.4 kN/m Show Supplier Material materials with Reißfestigkeit of 20.4 kN/m | ASTM D624 Die C | 500 mm/min |
Zugfestigkeit | 3.4 MPa Show Supplier Material materials with Zugfestigkeit of 3.4 MPa | ASTM D412 | 500 mm/min |
Rheological Properties
Property | Value | Testing Standard | Comment |
---|---|---|---|
Schmelzmassenflussrate | 10.9 g/10min Show Supplier Material materials with Schmelzmassenflussrate of 10.9 g/10min | ASTM D1238 | 190°C/2.16kg |
Schrumpfung | 0.8 - 1.4 % Show Supplier Material materials with Schrumpfung of 0.8 - 1.4 % | ASTM D955 | Transverse |
1 - 1.6 % Show Supplier Material materials with Schrumpfung of 1 - 1.6 % | ASTM D955 |
Technological properties
Property | ||
---|---|---|
Application areas | Massage ball | |
Certifications | REACH SVHC free, RoHS 2.0, GS AfPS GS 2019:01 PAK, EN 71-3 | |
Color | White | |
Fillers | Calcium Carbonate | |
Other | Overmolding capabilities: PP |