Allgemein
Property | Value | Testing Standard |
---|---|---|
Dichte | 0.85 - 0.91 g/cm³ Show Supplier Material materials with Dichte of 0.85 - 0.91 g/cm³ | ASTM D792 |
Mechanisch
Property | Temperature | Value | Testing Standard | Comment |
---|---|---|---|---|
Dehnung | 719.6 % Show Supplier Material materials with Dehnung of 719.6 % | ASTM D412 | 500 mm/min | |
Druckverformungsrest | 23 °C | 17.5 [-] Show Supplier Material materials with Druckverformungsrest of 17.5 [-] | ASTM D395 B | |
70 °C | 64.6 [-] Show Supplier Material materials with Druckverformungsrest of 64.6 [-] | ASTM D395 B | ||
Härte, Shore A | 37 - 43 [-] Show Supplier Material materials with Härte, Shore A of 37 - 43 [-] | ASTM D2240 | ||
Modul bei 100 % Dehnung | 0.00085 GPa Show Supplier Material materials with Modul bei 100 % Dehnung of 0.00085 GPa | ASTM D412 | 500 mm/min | |
Modul bei 300 % Dehnung | 0.00144 GPa Show Supplier Material materials with Modul bei 300 % Dehnung of 0.00144 GPa | ASTM D412 | 500 mm/min | |
Reißfestigkeit | 14.4 kN/m Show Supplier Material materials with Reißfestigkeit of 14.4 kN/m | ASTM D624 Die C | 500 mm/min | |
Zugfestigkeit | 3.0 MPa Show Supplier Material materials with Zugfestigkeit of 3.0 MPa | ASTM D412 | 500 mm/min |
Rheological Properties
Property | Value | Testing Standard | Comment |
---|---|---|---|
Schmelzmassenflussrate | 15.3 g/10min Show Supplier Material materials with Schmelzmassenflussrate of 15.3 g/10min | ASTM D1238 | 190°C/2.16kg |
Schrumpfung | 1.4 - 2 % Show Supplier Material materials with Schrumpfung of 1.4 - 2 % | ASTM D955 | Transverse |
1.5 - 2.1 % Show Supplier Material materials with Schrumpfung of 1.5 - 2.1 % | ASTM D955 |
Technological properties
Property | ||
---|---|---|
Application areas | Sports, toothbrush, seal | |
Certifications | REACH SVHC free, RoHS 2.0, GS AfPS GS 2019:01 PAK, EN 71-3, Meets FDA requirements | |
Color | Translucent | |