Allgemein
Property | Value | Condition | Testing Standard |
---|---|---|---|
Dichte | 1.29 g/cm³ Show Supplier Material materials with Dichte of 1.29 g/cm³ | dry | ISO 1183 |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Biegefestigkeit | 171 MPa Show Supplier Material materials with Biegefestigkeit of 171 MPa | dry | ISO 178 | 2mm/min | |
Biegemodul | 6.2 GPa Show Supplier Material materials with Biegemodul of 6.2 GPa | dry | ISO 178 | 2mm/min | |
Dehnung | 2.9 % Show Supplier Material materials with Dehnung of 2.9 % | dry | ISO 527-2/1A | 5mm/min | |
Elastizitätsmodul | 7.1 GPa Show Supplier Material materials with Elastizitätsmodul of 7.1 GPa | dry | ISO 527-2/1A | 1mm/min | |
Schlagfestigkeit, Charpy gekerbt | 23 °C | 7.2 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 7.2 kJ/m² | dry | ISO 179/1eA | |
Schlagzähigkeit, Charpy ungekerbt | 23 °C | 49 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 49 kJ/m² | dry | ISO 179/1eU | |
Zugfestigkeit | 113 MPa Show Supplier Material materials with Zugfestigkeit of 113 MPa | dry | ISO 527-2/1A | 5mm/min |
Thermisch
Property | Value | Testing Standard | Comment | ||
---|---|---|---|---|---|
Schmelzpunkt | 260 °C Show Supplier Material materials with Schmelzpunkt of 260 °C | ISO 11357-1/-3 | 10°C/min | ||
Vicat-Erweichungstemperatur | 220 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 220 °C | ISO 306 | 50°C/h 50N | ||
Wärmeformbeständigkeitstemperatur | 215 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 215 °C | ISO 75/2Af | 1.80 MPa | ||
250 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 250 °C | ISO 75/2Bf | 0.45 MPa | |||
Entflammbarkeit | Thickness tested (mm): 0.8, Class: V-0, Standard: UL 94 |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Surface resistivity | 1e+10 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+10 Ω/sq | 50%RH | IEC 60093 | 500V |
1e+12 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+12 Ω/sq | dry | IEC 60093 | 500V | |
Volume resistivity | 1e+11 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+11 Ω·cm | 50%RH | IEC 60093 | 500V |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 60093 | 500V |
Rheological Properties
Property | Value | Testing Standard | Comment |
---|---|---|---|
Schmelzmassenflussrate | 32 g/10min Show Supplier Material materials with Schmelzmassenflussrate of 32 g/10min | ISO 1133 | 275°C/3.25Kg |
Technological properties
Property | ||
---|---|---|
Certifications | RoHS 2011/65/UE | |
Color | Black | |
Features | Flame Retardant, Halogen-free, Heat Stabilized | |
Fillers | 15% Glass Fiber | |
Processing methods | Injection Molding |