Allgemein
Property | Temperature | Value | Condition | Testing Standard | Thickness | Comment |
---|---|---|---|---|---|---|
Dichte | 1.63 g/cm³ Show Supplier Material materials with Dichte of 1.63 g/cm³ | dry | ISO 1183 | |||
Moisture absorption | 23 °C | 0.9 % Show Supplier Material materials with Moisture absorption of 0.9 % | 50%RH | ISO 62 | 2 mm | |
Wasserabsorption | 3.2 % Show Supplier Material materials with Wasserabsorption of 3.2 % | ISO 62 | 2 mm | immersion at 23°C |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Biegefestigkeit | 170 MPa Show Supplier Material materials with Biegefestigkeit of 170 MPa | dry | ISO 178 | 2mm/min | |
Biegemodul | 10.2 GPa Show Supplier Material materials with Biegemodul of 10.2 GPa | dry | ISO 178 | 2mm/min | |
Dehnung | 1.8 % Show Supplier Material materials with Dehnung of 1.8 % | dry | ISO 527-2/1A | 5mm/min | |
Elastizitätsmodul | 11 GPa Show Supplier Material materials with Elastizitätsmodul of 11 GPa | dry | ISO 527-2/1A | 1mm/min | |
Schlagzähigkeit, Charpy ungekerbt | 23 °C | 35 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 35 kJ/m² | dry | ISO 179/1eU | |
Zugfestigkeit | 120 MPa Show Supplier Material materials with Zugfestigkeit of 120 MPa | dry | ISO 527-2/1A | 5mm/min |
Thermisch
Property | Value | Thickness | Testing Standard | Comment | |||
---|---|---|---|---|---|---|---|
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | 1 mm, 2 mm | IEC 60695-2-12 | ||||
Glow Wire Ignition Temperature | 775 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 775 °C | 1 mm, 2 mm | IEC 60695-2-13 | ||||
Schmelzpunkt | 220 °C Show Supplier Material materials with Schmelzpunkt of 220 °C | ISO 11357-1/-3 | 10°C/min | ||||
Vicat-Erweichungstemperatur | 200 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 200 °C | ISO 306 | 1.00E+12mm | ||||
Wärmeformbeständigkeitstemperatur | 205 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 205 °C | ISO 75/2Af | 1.80 MPa | ||||
Entflammbarkeit | Class: V-0, Standard: UL 94 | Automotive Interior Flammability(mm/min): 0 ,method: ISO 3795 and thickness tested (mm): 3 |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Kriechstromfestigkeit | 350 V Show Supplier Material materials with Kriechstromfestigkeit of 350 V | dry | IEC 60112 | Sol.A |
Volume resistivity | 1e+11 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+11 Ω·cm | 50%RH | IEC 60093 | 500V |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 60093 | 500V |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Schrumpfung | 0.2 % Show Supplier Material materials with Schrumpfung of 0.2 % | 270/80/60* | ISO 294-4 | *Melt Temp. [°C] / Mold Temp. [°C] / Cavity Press. [MPa] |
0.5 % Show Supplier Material materials with Schrumpfung of 0.5 % | 270/80/60* | ISO 294-4 | *Melt Temp. [°C] / Mold Temp. [°C] / Cavity Press. [MPa], Transverse |
Technological properties
Property | ||
---|---|---|
Additives | Release agent, Flame retarding agent | |
Certifications | RoHS 2011/65/UE | |
Color | Black | |
Features | Flame Retardant, Heat Stabilized | |
Fillers | 30% Glass Fiber | |
Processing methods | Injection Molding |