Allgemein
Property | Temperature | Value | Condition | Testing Standard | Thickness | Comment |
---|---|---|---|---|---|---|
Dichte | 1.4 g/cm³ Show Supplier Material materials with Dichte of 1.4 g/cm³ | dry | ISO 1183 | |||
Moisture absorption | 23 °C | 1.5 % Show Supplier Material materials with Moisture absorption of 1.5 % | 50%RH | ISO 62 | 2 mm | |
Wasserabsorption | 6.3 % Show Supplier Material materials with Wasserabsorption of 6.3 % | ISO 62 | 2 mm | immersion at 23°C |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Biegefestigkeit | 290 MPa Show Supplier Material materials with Biegefestigkeit of 290 MPa | dry | ISO 178 | 2mm/min | |
Biegemodul | 9 GPa Show Supplier Material materials with Biegemodul of 9 GPa | dry | ISO 178 | 2mm/min | |
Dehnung | 3.5 % Show Supplier Material materials with Dehnung of 3.5 % | 50%RH | ISO 527-2/1A | 5mm/min | |
3.7 % Show Supplier Material materials with Dehnung of 3.7 % | dry | ISO 527-2/1A | 5mm/min | ||
Elastizitätsmodul | 10 GPa Show Supplier Material materials with Elastizitätsmodul of 10 GPa | 50%RH | ISO 527-2/1A | 1mm/min | |
10.3 GPa Show Supplier Material materials with Elastizitätsmodul of 10.3 GPa | dry | ISO 527-2/1A | 1mm/min | ||
Schlagfestigkeit, Charpy gekerbt | -30 °C | 8.5 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 8.5 kJ/m² | dry | ISO 179/1eA | |
23 °C | 10.5 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 10.5 kJ/m² | dry | ISO 179/1eA | ||
23 °C | 14.5 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 14.5 kJ/m² | 50%RH | ISO 179/1eA | ||
Schlagzähigkeit, Charpy ungekerbt | -30 °C | 87 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 87 kJ/m² | dry | ISO 179/1eU | |
23 °C | 100 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 100 kJ/m² | dry | ISO 179/1eU | ||
23 °C | 102 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 102 kJ/m² | 50%RH | ISO 179/1eU | ||
Zugfestigkeit | 130 MPa Show Supplier Material materials with Zugfestigkeit of 130 MPa | 50%RH | ISO 527-2/1A | 5mm/min | |
195 MPa Show Supplier Material materials with Zugfestigkeit of 195 MPa | dry | ISO 527-2/1A | 5mm/min |
Thermisch
Property | Value | Thickness | Testing Standard | Comment | |||
---|---|---|---|---|---|---|---|
Glow Wire Flammability Index | 700 °C Show Supplier Material materials with Glow Wire Flammability Index of 700 °C | 2 mm | IEC 60695-2-12 | ||||
Schmelzpunkt | 260 °C Show Supplier Material materials with Schmelzpunkt of 260 °C | ISO 11357-1/-3 | 10°C/min | ||||
Vicat-Erweichungstemperatur | 250 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 250 °C | ISO 306 | 50°C/h 50N | ||||
Wärmeformbeständigkeitstemperatur | 235 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 235 °C | ISO 75/2Af | 1.80 MPa | ||||
250 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 250 °C | ISO 75/2Bf | 0.45 MPa | |||||
Entflammbarkeit | Thickness tested (mm): 0.8, Class: HB, Standard: UL 94 | Automotive Interior Flammability(mm/min): 0 ,method: ISO 3795 and thickness tested (mm): 3 |
Elektrisch
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Kriechstromfestigkeit | 550 V Show Supplier Material materials with Kriechstromfestigkeit of 550 V | dry | IEC 60112 | Sol.A |
Surface resistivity | 1e+10 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+10 Ω/sq | 50%RH | IEC 60093 | 500V |
1e+12 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+12 Ω/sq | dry | IEC 60093 | 500V | |
Volume resistivity | 1e+11 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+11 Ω·cm | 50%RH | IEC 60093 | 500V |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 60093 | 500V |
Technological properties
Property | ||
---|---|---|
Additives | Release agent | |
Certifications | Yellow Card, RoHS 2011/65/UE | |
Color | Natural | |
Fillers | 35% Glass Fiber | |
Processing methods | Injection Molding |