Allgemein
Property | Temperature | Value | Condition | Testing Standard | Thickness | Comment |
---|---|---|---|---|---|---|
Dichte | 1.36 g/cm³ Show Supplier Material materials with Dichte of 1.36 g/cm³ | dry | ISO 1183 | |||
Moisture absorption | 23 °C | 2 % Show Supplier Material materials with Moisture absorption of 2 % | 50%RH | ISO 62 | 2 mm | |
Wasserabsorption | 7.5 % Show Supplier Material materials with Wasserabsorption of 7.5 % | ISO 62 | 2 mm | immersion at 23°C |
Mechanisch
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Biegefestigkeit | 160 MPa Show Supplier Material materials with Biegefestigkeit of 160 MPa | 50%RH | ISO 178 | 2mm/min | |
225 MPa Show Supplier Material materials with Biegefestigkeit of 225 MPa | dry | ISO 178 | 2mm/min | ||
Biegemodul | 6.1 GPa Show Supplier Material materials with Biegemodul of 6.1 GPa | 50%RH | ISO 178 | 2mm/min | |
7.7 GPa Show Supplier Material materials with Biegemodul of 7.7 GPa | dry | ISO 178 | 2mm/min | ||
Dehnung | 3.4 % Show Supplier Material materials with Dehnung of 3.4 % | dry | ISO 527-2/1A | 5mm/min | |
6.5 % Show Supplier Material materials with Dehnung of 6.5 % | 50%RH | ISO 527-2/1A | 5mm/min | ||
Elastizitätsmodul | 6.5 GPa Show Supplier Material materials with Elastizitätsmodul of 6.5 GPa | 50%RH | ISO 527-2/1A | 1mm/min | |
9.5 GPa Show Supplier Material materials with Elastizitätsmodul of 9.5 GPa | dry | ISO 527-2/1A | 1mm/min | ||
Schlagfestigkeit, Charpy gekerbt | 23 °C | 10 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 10 kJ/m² | dry | ISO 179/1eA | |
23 °C | 15 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 15 kJ/m² | 50%RH | ISO 179/1eA | ||
Schlagzähigkeit, Charpy ungekerbt | 75 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 75 kJ/m² | dry | ISO 179/1eU | 23°C | |
85 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Charpy ungekerbt of 85 kJ/m² | 50%RH | ISO 179/1eU | 23°C | ||
Zugfestigkeit | 105 MPa Show Supplier Material materials with Zugfestigkeit of 105 MPa | 50%RH | ISO 527-2/1A | 5mm/min | |
150 MPa Show Supplier Material materials with Zugfestigkeit of 150 MPa | dry | ISO 527-2/1A | 5mm/min |
Thermisch
Property | Value | Testing Standard | Comment |
---|---|---|---|
Schmelzpunkt | 219 °C Show Supplier Material materials with Schmelzpunkt of 219 °C | ISO 11357-1/-3 | 10°C/min |
Technological properties
Property | ||
---|---|---|
Additives | Release agent | |
Certifications | RoHS 2011/65/UE | |
Color | Black | |
Fillers | 30% Glass Fiber | |
Processing methods | Injection Molding |