Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 1.27 g/cm³ Show Supplier Material materials with Dichte of 1.27 g/cm³ | ASTM D 792 |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegefestigkeit | 23.0 °C | 206 MPa Show Supplier Material materials with Biegefestigkeit of 206 MPa | ISO 178 |
Biegemodul | 23.0 °C | 16.5 GPa Show Supplier Material materials with Biegemodul of 16.5 GPa | ISO 178 | 2 mm/min |
Dehnung | 23.0 °C | 1 % Show Supplier Material materials with Dehnung of 1 % | ISO 527 | break, 5 mm/min |
Elastizitätsmodul | 23.0 °C | 19.4 GPa Show Supplier Material materials with Elastizitätsmodul of 19.4 GPa | ISO 527 | 1 mm/min |
Impact strength, Izod notched, ASTM | 23.0 °C | 117 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 117 J/m | ASTM D 256 | notched, 23°C |
Impact strength, Izod unnotched, ASTM | 23.0 °C | 694 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 694 J/m | ASTM D 4812 | 23°C |
Schlagzähigkeit, Izod gekerbt | 23.0 °C | 129 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Izod gekerbt of 129 kJ/m² | ISO 180/1A | 80*10*4, 23°C |
Zugfestigkeit | 23.0 °C | 130 MPa Show Supplier Material materials with Zugfestigkeit of 130 MPa | ISO 527 | break, 5 mm/min |
Thermisch
Property | Value | Comment |
---|---|---|
Heat deflection temperature, 1.80 MPa | 170 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 170 °C | ISO 75/Af | Flatw 80*10*4 sp=64mm |
Wärmeformbeständigkeitstemperatur | 170 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 170 °C |
Technological properties
Property | ||
---|---|---|
Application areas | Auto Aftermarket | |
Availability | Asia,Americas | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |