Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Relative Dichte | 23.0 °C | 1.11 [-] Show Supplier Material materials with Relative Dichte of 1.11 [-] | ASTM D 792 | |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegefestigkeit | 23.0 °C | 99 MPa Show Supplier Material materials with Biegefestigkeit of 99 MPa | ASTM D 790 | yld, 2.6 mm/min, 100 mm span |
Biegemodul | 23.0 °C | 2.5 GPa Show Supplier Material materials with Biegemodul of 2.5 GPa | ASTM D 790 | 2.6 mm/min, 100 mm span |
Dehnung | 23.0 °C | 17 % Show Supplier Material materials with Dehnung of 17 % | ASTM D 638 | brk, Type I, 50 mm/min |
Impact strength, Izod notched, ASTM | 23.0 °C | 96 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 96 J/m | ASTM D 256 | notched, -30°C |
Instrumented Impact, at Peak | 23.0 °C | 39 J Show Supplier Material materials with Instrumented Impact, at Peak of 39 J | ASTM D 3763 | 23°C |
Schlagzähigkeit, Izod gekerbt | 23.0 °C | 186 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Izod gekerbt of 186 kJ/m² | ASTM D 256 | notched, 23°C |
Zugfestigkeit | 23.0 °C | 66 MPa Show Supplier Material materials with Zugfestigkeit of 66 MPa | ASTM D 638 | yld, Type I, 50 mm/min |
Thermisch
Property | Value | Comment | |
---|---|---|---|
Heat deflection temperature, 0.45 MPa | 109 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 109 °C | ASTM D 648 | 6.4 mm, unannealed | |
Heat deflection temperature, 1.80 MPa | 99 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 99 °C | ASTM D 648 | 6.4 mm, unannealed | |
Relative temperature index, electrical | 95 °C Show Supplier Material materials with Relative temperature index, electrical of 95 °C | UL 746B | |
Relative temperature index, mechanical impact | 80 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 80 °C | UL 746B | |
Relative temperature index, mechanical strength | 95 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 95 °C | UL 746B | |
Vicat-Erweichungstemperatur | 128 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 128 °C | ASTM D 1525 | Rate B/50 | |
Wärmeformbeständigkeitstemperatur | 99 - 109 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 99 - 109 °C | ||
Entflammbarkeit | UL Recognized, 94HB Flame Class Rating: ≥0.4mm UL 94 <br> Radiant Panel Listing: TRUE- UL Tested <br> UL Recognized, 94V-0 Flame Class Rating: ≥1.5mm UL 94 <br> UL Recognized, 94-5VA Flame Class Rating: ≥3mm UL 94 <br> UV-light, water exposure/immersion: F1- UL 746C <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=221178- - |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dielectric constant, 60Hz | 23.0 °C | 2.69 [-] Show Supplier Material materials with Dielectric constant, 60Hz of 2.69 [-] | ASTM D 150 | 50/60 Hz |
Dielektrizitätskonstante, 1 MHz | 23.0 °C | 2.55 [-] Show Supplier Material materials with Dielektrizitätskonstante, 1 MHz of 2.55 [-] | ASTM D 150 |
Dissipation factor, 1MHz | 23.0 °C | 7E-3 [-] Show Supplier Material materials with Dissipation factor, 1MHz of 7E-3 [-] | ASTM D 150 |
Dissipation factor, 50Hz | 23.0 °C | 0.01 [-] Show Supplier Material materials with Dissipation factor, 50Hz of 0.01 [-] | ASTM D 150 | 50/60 Hz |
Durchschlagfestigkeit | 23.0 °C | 16.2 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 16.2 kV/mm | ASTM D 149 | in oil, 3.2 mm |
High Amp Arc Ignition | 23.0 °C | 1.5 mm Show Supplier Material materials with High Amp Arc Ignition of 1.5 mm | ≥, UL 746A | PLC 0 |
High Volt Arc Track Rate | 23.0 °C | 4 PLC Code Show Supplier Material materials with High Volt Arc Track Rate of 4 PLC Code | UL 746A | (PLC) |
Hot-Wire Ignition | 23.0 °C | 6 mm Show Supplier Material materials with Hot-Wire Ignition of 6 mm | ≥, UL 746A | PLC 0 |
Kriechstromfestigkeit | 23.0 °C | 1 V Show Supplier Material materials with Kriechstromfestigkeit of 1 V | UL 746A | (UL) {PLC} |
Sheet resistivity, ROA | 23.0 °C | 1.00E+14 Ω Show Supplier Material materials with Sheet resistivity, ROA of 1.00E+14 Ω | >, ASTM D 257 |
Volume resistivity | 23.0 °C | 2.80E+16 Ω·cm Show Supplier Material materials with Volume resistivity of 2.80E+16 Ω·cm | ASTM D 257 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | EV/HEV Battery, Food Processor, Enclosures, Electronic Components, Circuit Protection, Data Management, Data Transfer, Document Handling, Meter Gas, Respiratory, Security/Detection, Small Appliance, Power Manangement, Wiring Devices, Wireless Communications | |
Availability | Americas | |
Processing methods | Maximum Moisture Content: 0.02% | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |