Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 1.27 g/cm³ Show Supplier Material materials with Dichte of 1.27 g/cm³ | ISO 1183 |
Moisture absorption | 23.0 °C | 0.7 % Show Supplier Material materials with Moisture absorption of 0.7 % | ISO 62 | (23°C / 50% RH) |
Relative Dichte | 23.0 °C | 1.27 [-] Show Supplier Material materials with Relative Dichte of 1.27 [-] | ASTM D 792 | |
Sauerstoffindex | 23.0 °C | 44 % Show Supplier Material materials with Sauerstoffindex of 44 % | |
Wasserabsorption | 23.0 °C | 1.25 % Show Supplier Material materials with Wasserabsorption of 1.25 % | ISO 62-1 | (23°C/saturated) |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegefestigkeit | 23.0 °C | 160 MPa Show Supplier Material materials with Biegefestigkeit of 160 MPa | ISO 178 | yield, 2 mm/min |
Biegemodul | 23.0 °C | 3.3 GPa Show Supplier Material materials with Biegemodul of 3.3 GPa | ISO 178 | 2 mm/min |
Dehnung | 23.0 °C | 6 % Show Supplier Material materials with Dehnung of 6 % | ISO 527 | yield, 5 mm/min |
Elastizitätsmodul | 23.0 °C | 3.2 GPa Show Supplier Material materials with Elastizitätsmodul of 3.2 GPa | ISO 527 | 1 mm/min |
Härte, Rockwell M | 23.0 °C | 109 [-] Show Supplier Material materials with Härte, Rockwell M of 109 [-] | ASTM D 785 | |
Impact strength, Izod notched, ASTM | 23.0 °C | 30 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 30 J/m | ASTM D 256 |
Impact strength, Izod unnotched, ASTM | 23.0 °C | 1335 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 1335 J/m | ASTM D 4812 | 23°C |
Instrumented Impact, Total Energy | 23.0 °C | 38 J Show Supplier Material materials with Instrumented Impact, Total Energy of 38 J | ASTM D 3763 | 23°C |
Schlagfestigkeit, Charpy gekerbt | 23.0 °C | 5 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 5 kJ/m² | ISO 179/1eA | V-notch Edgew, 23°C, 80*10*4 sp=62mm |
Schlagzähigkeit, Izod gekerbt | 23.0 °C | 32 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Izod gekerbt of 32 kJ/m² | ASTM D 256 | notched, 23°C |
Taber Abrasion | 23.0 °C | 10 mg/1000cy Show Supplier Material materials with Taber Abrasion of 10 mg/1000cy | ASTM D 1044 | CS-17, 1 kg |
Zugfestigkeit | 23.0 °C | 105 MPa Show Supplier Material materials with Zugfestigkeit of 105 MPa | ISO 527 | yield, 5 mm/min |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Ball Pressure Test | Passes | IEC 60695-10-2 | 75°C +/- 2°C | |
Heat deflection temperature, 0.45 MPa | 207 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 207 °C | ASTM D 648 | 6.4 mm, unannealed | |
Heat deflection temperature, 1.80 MPa | 190 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 190 °C | ISO 75/Af | Flatw 80*10*4 sp=64mm | |
Koeffizient der thermischen Ausdehnung | 23.0 °C | 5.5E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 5.5E-5 1/K | ISO 11359-2 | -40°C to 40°C |
Vicat-Erweichungstemperatur | 211 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 211 °C | ISO 306 | Rate B/50 | |
Wärmeformbeständigkeitstemperatur | 190 - 207 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 190 - 207 °C | ||
Wärmeleitfähigkeit | 23.0 °C | 0.22 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 0.22 W/(m·K) | ASTM C177 |
thermischer Ausdehnungskoeffizient, transversal | 23.0 °C | 5.5E-5 1/K Show Supplier Material materials with thermischer Ausdehnungskoeffizient, transversal of 5.5E-5 1/K | ISO 11359-2 | -40°C to 40°C |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dissipation factor, 1kHz | 23.0 °C | 1.3E-3 [-] Show Supplier Material materials with Dissipation factor, 1kHz of 1.3E-3 [-] | ASTM D 150 |
Durchschlagfestigkeit | 23.0 °C | 32.6 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 32.6 kV/mm | ASTM D 149 | in air, 1.6 mm |
Verlustfaktor | 23.0 °C | 2.5E-3 [-] Show Supplier Material materials with Verlustfaktor of 2.5E-3 [-] | ASTM D 150 | 2450 MHz |
Volume resistivity | 23.0 °C | 1.00E+17 Ω·cm Show Supplier Material materials with Volume resistivity of 1.00E+17 Ω·cm | ASTM D 257 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Schmelzmassenflussrate | 17.8 g/10min Show Supplier Material materials with Schmelzmassenflussrate of 17.8 g/10min | ASTM D 1238 | 337°C/6.6 kgf | |
Schmelzvolumenflussrate | 13 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 13 cm³/10min | ISO 1133 | MVR at 340°C/5.0 kg | |
Schrumpfung | 23.0 °C | 0.5 % Show Supplier Material materials with Schrumpfung of 0.5 % | SABIC method | 3.2 mm |
Technological properties
Property | ||
---|---|---|
Application areas | Water Treatment/Filtration | |
Availability | Americas | |
Processing methods | Middle - Zone 2 Temperature: 340 to 400.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |