Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Relative Dichte | 23.0 °C | 1.25 [-] Show Supplier Material materials with Relative Dichte of 1.25 [-] | ASTM D 792 | |
Sauerstoffindex | 23.0 °C | 30 % Show Supplier Material materials with Sauerstoffindex of 30 % | |
Wasserabsorption | 23.0 °C | 0.22 % Show Supplier Material materials with Wasserabsorption of 0.22 % | ISO 62-1 | (23°C/saturated) |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegefestigkeit | 23.0 °C | 125 MPa Show Supplier Material materials with Biegefestigkeit of 125 MPa | ISO 178 | break, 2 mm/min |
Biegemodul | 23.0 °C | 4.5 GPa Show Supplier Material materials with Biegemodul of 4.5 GPa | ISO 178 | 2 mm/min |
Dehnung | 23.0 °C | 2 % Show Supplier Material materials with Dehnung of 2 % | ISO 527 | break, 5 mm/min |
Zugfestigkeit | 23.0 °C | 80 MPa Show Supplier Material materials with Zugfestigkeit of 80 MPa | ISO 527 | break, 5 mm/min |
Thermisch
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Heat deflection temperature, 0.45 MPa | 135 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 135 °C | ISO 75/Be | Edgew 120*10*4 sp=100mm | |||
Heat deflection temperature, 1.80 MPa | 130 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 130 °C | ISO 75/Ae | Edgew 120*10*4 sp=100mm | |||
Koeffizient der thermischen Ausdehnung | 23.0 °C | 3E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 3E-5 1/K | ISO 11359-2 | 23°C to 80°C | ||
Relative temperature index, electrical | 110 °C Show Supplier Material materials with Relative temperature index, electrical of 110 °C | UL 746B | |||
Relative temperature index, mechanical impact | 105 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 105 °C | UL 746B | |||
Relative temperature index, mechanical strength | 110 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 110 °C | UL 746B | |||
Wärmeformbeständigkeitstemperatur | 130 - 135 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 130 - 135 °C | ||||
Entflammbarkeit | UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=104212941- - <br> UL Recognized, 94-5VA Flame Class Rating: ≥2mm UL 94 <br> UL Recognized, 94V-0 Flame Class Rating: ≥6mm UL 94 <br> UL Recognized, 94V-1 Flame Class Rating: ≥1.5mm UL 94 <br> Glow Wire Flammability Index, 1.0 mm: 960°C IEC 60695-2-12 <br> Glow Wire Ignitability Temperature, 1.0 mm: 800°C IEC 60695-2-13 <br> UV-light, water exposure/immersion: F2- UL 746C |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dielectric constant, 60Hz | 23.0 °C | 3 [-] Show Supplier Material materials with Dielectric constant, 60Hz of 3 [-] | IEC 60250 | 50/60 Hz |
Dissipation factor, 50Hz | 23.0 °C | 4E-3 [-] Show Supplier Material materials with Dissipation factor, 50Hz of 4E-3 [-] | IEC 60250 | 50/60 Hz |
Durchschlagfestigkeit | 23.0 °C | 30 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 30 kV/mm | IEC 60243-1 | in oil, 0.8 mm |
High Amp Arc Ignition | 23.0 °C | 1 mm Show Supplier Material materials with High Amp Arc Ignition of 1 mm | UL 746A | surface {PLC} |
High Volt Arc Track Rate | 23.0 °C | 4 PLC Code Show Supplier Material materials with High Volt Arc Track Rate of 4 PLC Code | UL 746A | (PLC) |
Hot-Wire Ignition | 23.0 °C | 0 mm Show Supplier Material materials with Hot-Wire Ignition of 0 mm | UL 746A | (PLC) |
Kriechstromfestigkeit | 23.0 °C | 3 V Show Supplier Material materials with Kriechstromfestigkeit of 3 V | UL 746A | (UL) {PLC} |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Schrumpfung | 23.0 °C | 0.2 % Show Supplier Material materials with Schrumpfung of 0.2 % | SABIC method | 3.2 mm |
Technological properties
Property | ||
---|---|---|
Application areas | Enclosure/Housing/Cover, Energy Management, Electronics, Enclosures, Electronic Components, EV Infrastructure, Electronic Material Handling, EV/HEV Battery, Fixture Bath/Shower, Industrial Material Handling, Individual Equiptment, Hygiene/Personal Care, HVAC Underhood, Lab Ware and Clinical Diagnostics, Hot Water System, Humidity Control, Heavy Vehicles, Cluster, Coffee Maker/Espresso Machine, Battery System, Building Element, Data Transfer, Document Handling, Displays, Dishwasher, Defense Vehicles, Drain Pan, Air Conditioning, Battery Pack, Building Accessory, Circuit Protection, Audio, Auto Aftermarket, ATM/Ticket Machine, Security/Detection, Respiratory, Sensor, Surgical Devices, Pump, Pipe/Fitting, Power Manangement, Plumbing, Photovoltaic Components, Ignition System, Meter Gas, Microwave Oven, Personal Computing, Non-LED Lighting, Motorcycle, Wearables, Water Treatment/Filtration, Wiring Devices, Wireless Communications, Washing Machine, Travel Suitcase, Swimming Pool/Spa, Traffic Management | |
Availability | Europe,Asia,Americas | |
Processing methods | Drying Temperature: 100 to 120.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |