Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegefestigkeit | 23.0 °C | 145 MPa Show Supplier Material materials with Biegefestigkeit of 145 MPa | ASTM D 790 | yld, 1.3 mm/min, 50 mm span |
Biegemodul | 23.0 °C | 4.1 GPa Show Supplier Material materials with Biegemodul of 4.1 GPa | ASTM D 790 | 1.3 mm/min, 50 mm span |
Impact strength, Izod notched, ASTM | 23.0 °C | 65 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 65 J/m | ASTM D 256 |
Impact strength, Izod unnotched, ASTM | 23.0 °C | 610 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 610 J/m | ASTM D 4812 | 23°C |
Schlagzähigkeit, Izod gekerbt | 23.0 °C | 65 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Izod gekerbt of 65 kJ/m² | ASTM D 256 | notched, 23°C |
Zugfestigkeit | 23.0 °C | 103 MPa Show Supplier Material materials with Zugfestigkeit of 103 MPa | ASTM D 638 | brk, Type I, 50 mm/min |
Thermisch
Property | Value | Comment |
---|---|---|
Heat deflection temperature, 0.45 MPa | 215 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 215 °C | ASTM D 648 | 3.2 mm, unannealed |
Heat deflection temperature, 1.80 MPa | 197 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 197 °C | ASTM D 648 | 3.2mm, unannealed |
Vicat-Erweichungstemperatur | 201 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 201 °C | ASTM D 1525 | Rate B/50 |
Wärmeformbeständigkeitstemperatur | 197 - 215 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 197 - 215 °C |
Technological properties
Property | ||
---|---|---|
Application areas | Enclosures | |
Availability | Europe,Asia,Americas | |
Processing methods | Drying Temperature: 100 to 110.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |