Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Wasserabsorption | 23.0 °C | 0.06 % Show Supplier Material materials with Wasserabsorption of 0.06 % | ASTM D 570 | (23°C/24hrs) |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegefestigkeit | 23.0 °C | 160 MPa Show Supplier Material materials with Biegefestigkeit of 160 MPa | ISO 178 | yield, 2 mm/min |
Biegemodul | 23.0 °C | 8.7 GPa Show Supplier Material materials with Biegemodul of 8.7 GPa | ISO 178 |
Dehnung | 23.0 °C | 1.8 % Show Supplier Material materials with Dehnung of 1.8 % | ISO 527 | break |
Elastizitätsmodul | 23.0 °C | 8.7 GPa Show Supplier Material materials with Elastizitätsmodul of 8.7 GPa | ISO 527 | 1 mm/min |
Schlagzähigkeit, Izod ungekerbt | 23.0 °C | 25 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Izod ungekerbt of 25 kJ/m² | ISO 180/1U | unnotched 80*10*4, 23°C |
Zugfestigkeit | 23.0 °C | 117 MPa Show Supplier Material materials with Zugfestigkeit of 117 MPa | ISO 527 | break |
Thermisch
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Heat deflection temperature, 0.45 MPa | 147 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 147 °C | ASTM D 648 | 3.2 mm, unannealed | |||
Heat deflection temperature, 1.80 MPa | 140 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 140 °C | ISO 75/Ae | Edgew 120*10*4 sp=100mm | |||
Koeffizient der thermischen Ausdehnung | 23.0 °C | 3.06E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 3.06E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Relative temperature index, electrical | 90 °C Show Supplier Material materials with Relative temperature index, electrical of 90 °C | UL 746B | |||
Relative temperature index, mechanical impact | 65 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C | UL 746B | |||
Relative temperature index, mechanical strength | 90 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 90 °C | UL 746B | |||
Vicat-Erweichungstemperatur | 147 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 147 °C | ISO 306 | Rate B/120 | |||
Wärmeformbeständigkeitstemperatur | 140 - 147 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 140 - 147 °C | ||||
thermischer Ausdehnungskoeffizient, transversal | 23.0 °C | 6.18E-5 1/K Show Supplier Material materials with thermischer Ausdehnungskoeffizient, transversal of 6.18E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Entflammbarkeit | UL Recognized, 94HB Flame Class Rating: ≥1.5mm UL 94 <br> UV-light, water exposure/immersion: F2- UL 746C <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=221162- - |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
Kriechstromfestigkeit | 23.0 °C | 250 V Show Supplier Material materials with Kriechstromfestigkeit of 250 V | IEC 60112 | |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Schmelzvolumenflussrate | 2 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 2 cm³/10min | ISO 1133 | MVR at 280°C/5.0 kg | |
Schrumpfung | 23.0 °C | 0.1 % Show Supplier Material materials with Schrumpfung of 0.1 % | SABIC method | 3.2 mm |
Technological properties
Property | ||
---|---|---|
Application areas | Auto Aftermarket, Circuit Protection, Building Accessory, Air Conditioning, Displays, Drain Pan, Dishwasher, Document Handling, Building Element, Bottles, Commercial Storage/Cookware, Data Management, Data Transfer, Electronic Components, Energy Management, Enclosure/Housing/Cover, Enclosures, Heavy Vehicles, Hot Water System, Lawn/Garden, Fixture Bath/Shower, Freezer, EV Infrastructure, Water Treatment/Filtration, Wiring Devices, Wireless Communications, Swimming Pool/Spa, Traffic Management, Washing Machine, Vending Machine, LED Lighting, Medical Device, Meter Gas, Ignition System, Medical Facility Infrastructure, Meter Water, Non-LED Lighting, Motorcycle, Personal Computing, Renal and Blood Handling, Semiconductor, Personal Water Craft, Small Appliance, Surgical Devices, Pipe/Fitting, Pump, Recreational Vehicle, Plumbing, Photovoltaic Components, Photo/Video Camera | |
Availability | Europe,Americas | |
Processing methods | Drying Temperature: 110 to 120.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |