Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of friction | 0.48 - 0.56 [-] Show Supplier Material materials with Coefficient of friction of 0.48 - 0.56 [-] | ||
Coefficient of friction, kinetic | 0.56 [-] Show Supplier Material materials with Coefficient of friction, kinetic of 0.56 [-] | ASTM D 3702 Modified: Manual | |
Coefficient of friction, static | 0.48 [-] Show Supplier Material materials with Coefficient of friction, static of 0.48 [-] | ASTM D 3702 Modified: Manual | |
Dichte | 23.0 °C | 1.48 g/cm³ Show Supplier Material materials with Dichte of 1.48 g/cm³ | ISO 1183 |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegefestigkeit | 23.0 °C | 195 MPa Show Supplier Material materials with Biegefestigkeit of 195 MPa | ASTM D 790 |
Biegemodul | 23.0 °C | 7.6 GPa Show Supplier Material materials with Biegemodul of 7.6 GPa | ASTM D 790 |
Schlagzähigkeit, Izod gekerbt | 23.0 °C | 12 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Izod gekerbt of 12 kJ/m² | ISO 180/1A | notched 80*10*4, 23°C |
Schlagzähigkeit, Izod ungekerbt | 23.0 °C | 80 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Izod ungekerbt of 80 kJ/m² | ISO 180/1U | 80*10*4, 23°C |
Thermisch
Property | Value | Comment | |
---|---|---|---|
Heat deflection temperature, 1.80 MPa | 236 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 236 °C | ISO 75/Af | Flatw 80*10*4 sp=64mm | |
Relative temperature index, electrical | 65 °C Show Supplier Material materials with Relative temperature index, electrical of 65 °C | UL 746B | |
Relative temperature index, mechanical impact | 65 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C | UL 746B | |
Relative temperature index, mechanical strength | 65 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 65 °C | UL 746B | |
Wärmeformbeständigkeitstemperatur | 236 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 236 °C | ||
Entflammbarkeit | UL Recognized, 94HB Flame Class Rating: ≥1.5mm UL 94 <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=101284272- - |
Technological properties
Property | ||
---|---|---|
Application areas | Furnace/Heater, Lawn/Garden, Electronic Components, Enclosures, Document Handling, Display, City, Travel Suitcase, Wiring Devices, Oil/Gas, Medical Device, Meter Gas | |
Availability | Europe,Asia,Americas | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |