Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegefestigkeit | 23.0 °C | 137 MPa Show Supplier Material materials with Biegefestigkeit of 137 MPa | ASTM D 790 | yld, 2.6 mm/min, 100 mm span |
Biegemodul | 23.0 °C | 3.1 GPa Show Supplier Material materials with Biegemodul of 3.1 GPa | ASTM D 790 | 2.6 mm/min, 100 mm span |
Dehnung | 23.0 °C | 60 % Show Supplier Material materials with Dehnung of 60 % | ASTM D 638 | brk, Type I, 5 mm/min |
Elastizitätsmodul | 23.0 °C | 2.9 GPa Show Supplier Material materials with Elastizitätsmodul of 2.9 GPa | ASTM D 638 | 5 mm/min |
Schlagzähigkeit, Izod gekerbt | 23.0 °C | 58 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Izod gekerbt of 58 kJ/m² | ASTM D 256 | notched, 23°C |
Zugfestigkeit | 23.0 °C | 99 MPa Show Supplier Material materials with Zugfestigkeit of 99 MPa | ASTM D 638 | yld, Type I, 5 mm/min |
Thermisch
Property | Value | Comment | |
---|---|---|---|
Heat deflection temperature, 1.80 MPa | 204 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 204 °C | ASTM D 648 | 6.4 mm, unannealed | |
Relative temperature index, electrical | 160 °C Show Supplier Material materials with Relative temperature index, electrical of 160 °C | UL 746B | |
Relative temperature index, mechanical impact | 155 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 155 °C | UL 746B | |
Relative temperature index, mechanical strength | 160 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 160 °C | UL 746B | |
Wärmeformbeständigkeitstemperatur | 204 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 204 °C | ||
Entflammbarkeit | UL Recognized, 94V-0 Flame Class Rating: ≥1.5mm UL 94 <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=221115- - |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dielectric constant, 60Hz | 23.0 °C | 3.2 [-] Show Supplier Material materials with Dielectric constant, 60Hz of 3.2 [-] | ASTM D 150 | 50/60 Hz |
Dissipation factor, 50Hz | 23.0 °C | 2.1E-3 [-] Show Supplier Material materials with Dissipation factor, 50Hz of 2.1E-3 [-] | ASTM D 150 | 50/60 Hz |
Durchschlagfestigkeit | 23.0 °C | 17.9 kV/mm Show Supplier Material materials with Durchschlagfestigkeit of 17.9 kV/mm | ASTM D 149 | in oil, 3.2 mm |
High Amp Arc Ignition | 23.0 °C | 1.5 mm Show Supplier Material materials with High Amp Arc Ignition of 1.5 mm | ≥, UL 746A | PLC 0 |
High Volt Arc Track Rate | 23.0 °C | 3 PLC Code Show Supplier Material materials with High Volt Arc Track Rate of 3 PLC Code | UL 746A | (PLC) |
Hot-Wire Ignition | 23.0 °C | 1.5 mm Show Supplier Material materials with Hot-Wire Ignition of 1.5 mm | ≥, UL 746A | PLC 1 |
Kriechstromfestigkeit | 23.0 °C | 4 V Show Supplier Material materials with Kriechstromfestigkeit of 4 V | UL 746A | (UL) {PLC} |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Schrumpfung | 23.0 °C | 0.5 % Show Supplier Material materials with Schrumpfung of 0.5 % | SABIC method | on tensile bar |
Technological properties
Property | ||
---|---|---|
Application areas | Fused Deposition Modeling (FDM), Enclosure/Housing/Cover, Electronic Components, Air Cabin Interiors, Aerospace, Aircraft Seating, Battery Cell, Data Transfer, Document Handling, Wireless Communications | |
Availability | Europe,Asia,Americas | |
Processing methods | Drying Temperature: 150°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |