Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegefestigkeit | 23.0 °C | 51 MPa Show Supplier Material materials with Biegefestigkeit of 51 MPa | ASTM D 790 | yld, 1.3 mm/min, 50 mm span |
Biegemodul | 23.0 °C | 1.6 GPa Show Supplier Material materials with Biegemodul of 1.6 GPa | ASTM D 790 | 1.3 mm/min, 50 mm span |
Dehnung | 23.0 °C | 195 % Show Supplier Material materials with Dehnung of 195 % | ASTM D 638 | brk, Type I, 50 mm/min |
Elastizitätsmodul | 23.0 °C | 1.3 GPa Show Supplier Material materials with Elastizitätsmodul of 1.3 GPa | ASTM D 638 | 50 mm/min |
Schlagzähigkeit, Izod gekerbt | 23.0 °C | 437 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Izod gekerbt of 437 kJ/m² | ASTM D 256 | notched, 23°C |
Zugfestigkeit | 23.0 °C | 32 MPa Show Supplier Material materials with Zugfestigkeit of 32 MPa | ASTM D 638 | brk, Type I, 50 mm/min |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Heat deflection temperature, 0.45 MPa | 113 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 113 °C | ASTM D 648 | 3.2 mm, unannealed | |
Heat deflection temperature, 1.80 MPa | 77 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 77 °C | ASTM D 648 | 3.2mm, unannealed | |
Koeffizient der thermischen Ausdehnung | 23.0 °C | 8.1E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 8.1E-5 1/K | ASTM E 831 | -40°C to 40°C |
Vicat-Erweichungstemperatur | 138 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 138 °C | ASTM D 1525 | Rate B/50 | |
Wärmeformbeständigkeitstemperatur | 77 - 113 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 77 - 113 °C | ||
thermischer Ausdehnungskoeffizient, transversal | 23.0 °C | 1.12E-4 1/K Show Supplier Material materials with thermischer Ausdehnungskoeffizient, transversal of 1.12E-4 1/K | ASTM E 831 | -40°C to 40°C |
Technological properties
Property | ||
---|---|---|
Application areas | Medical Device, Wiring Devices, Hot Water System, EV/HEV Battery, Document Handling | |
Availability | Europe,Asia,Americas | |
Processing methods | Nozzle Temperature: 260 to 290.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |