Allgemein
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegefestigkeit | 23.0 °C | 95 MPa Show Supplier Material materials with Biegefestigkeit of 95 MPa | ISO 178 | yield, 2 mm/min |
Biegemodul | 23.0 °C | 2.3 GPa Show Supplier Material materials with Biegemodul of 2.3 GPa | ISO 178 | 2 mm/min |
Dehnung | 23.0 °C | 70 % Show Supplier Material materials with Dehnung of 70 % | ISO 527 | break, 50 mm/min |
Elastizitätsmodul | 23.0 °C | 2.1 GPa Show Supplier Material materials with Elastizitätsmodul of 2.1 GPa | ISO 527 | 1 mm/min |
Schlagfestigkeit, Charpy gekerbt | 23.0 °C | 17 kJ/m² Show Supplier Material materials with Schlagfestigkeit, Charpy gekerbt of 17 kJ/m² | ISO 179/1eA | V-notch Edgew, 23°C, 80*10*4 sp=62mm |
Schlagzähigkeit, Izod gekerbt | 23.0 °C | 5 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Izod gekerbt of 5 kJ/m² | ISO 180/1A | 80*10*4, -30°C |
Zugfestigkeit | 23.0 °C | 57 MPa Show Supplier Material materials with Zugfestigkeit of 57 MPa | ISO 527 | yield, 50 mm/min |
Thermisch
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Heat deflection temperature, 1.80 MPa | 115 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 115 °C | ISO 75/Ae | Edgew 120*10*4 sp=100mm | |||
Koeffizient der thermischen Ausdehnung | 23.0 °C | 7.3E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 7.3E-5 1/K | ISO 11359-2 | -40°C to 40°C | ||
Relative temperature index, electrical | 105 °C Show Supplier Material materials with Relative temperature index, electrical of 105 °C | UL 746B | |||
Relative temperature index, mechanical impact | 90 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 90 °C | UL 746B | |||
Relative temperature index, mechanical strength | 105 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 105 °C | UL 746B | |||
Vicat-Erweichungstemperatur | 140 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 140 °C | ISO 306 | Rate B/120 | |||
Wärmeformbeständigkeitstemperatur | 115 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 115 °C | ||||
thermischer Ausdehnungskoeffizient, transversal | 23.0 °C | 8.3E-5 1/K Show Supplier Material materials with thermischer Ausdehnungskoeffizient, transversal of 8.3E-5 1/K | ISO 11359-2 | -40°C to 40°C | ||
Entflammbarkeit | UL Recognized, 94HB Flame Class Rating: ≥1.5mm UL 94 <br> UL Yellow Card Link: https://iq.ul.com/ul/cert.aspx?ULID=221150- - |
Elektrisch
Property | Temperature | Value | Comment |
---|---|---|---|
High Amp Arc Ignition | 23.0 °C | 6 mm Show Supplier Material materials with High Amp Arc Ignition of 6 mm | ≥, UL 746A | PLC 4 |
High Volt Arc Track Rate | 23.0 °C | 4 PLC Code Show Supplier Material materials with High Volt Arc Track Rate of 4 PLC Code | UL 746A | (PLC) |
Hot-Wire Ignition | 23.0 °C | 1.5 mm Show Supplier Material materials with Hot-Wire Ignition of 1.5 mm | ≥, UL 746A | PLC 1 |
Kriechstromfestigkeit | 23.0 °C | 3 V Show Supplier Material materials with Kriechstromfestigkeit of 3 V | UL 746A | (UL) {PLC} |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Schmelzvolumenflussrate | 12 cm³/10min Show Supplier Material materials with Schmelzvolumenflussrate of 12 cm³/10min | ISO 1133 | MVR at 280°C/5.0 kg | |
Schrumpfung | 23.0 °C | 0.5 % Show Supplier Material materials with Schrumpfung of 0.5 % | SABIC method | 3.2 mm |
Technological properties
Property | ||
---|---|---|
Application areas | Meter Gas, Ignition System, Monitoring and Imaging, Meter Water, Laundry Dryer, LED Lighting, Medical Device, Personal Computing, Non-LED Lighting, Sanitary, Small Appliance, Security/Detection, Renal and Blood Handling, Refrigerator, Recreational Vehicle, Power Boat, Pipe/Fitting, Pump, Plumbing, Pharmaceutical Packaging & Drug Delivery, Wireless Communications, Wiring Devices, Watch/Jewelry, Water Treatment/Filtration, Wheel Cover, Wearables, Swimming Pool/Spa, Surgical Tray, Vending Machine, Washing Machine, Auto Electrical, Building Accessory, Circuit Protection, Audio, Auto Aftermarket, ATM/Ticket Machine, Amusement Machine, Animal Testing, Aerospace, Coffee Maker/Espresso Machine, Bottles, Building Element, Building/Construction Sheet, Data Management, Doors Hardware/Trim, Conveyor, Dishwasher, Displays, Document Handling, EV Infrastructure, Food Transportation, Furnace/Heater, Fixture Bath/Shower, Lawn/Garden, Lab Ware and Clinical Diagnostics, Heavy Vehicles, Gas/Electric Oven, Hot Water System, Head Protection, Electronic Components, Enclosure/Housing/Cover, Electronics, Enclosures | |
Availability | Americas | |
Processing methods | Middle - Zone 2 Temperature: 260 to 305.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |