FLEX NORYL™ Resin WCA875 - Europe

Want to keep this datasheet? Save it now in your required format

Description

FLEX NORYL™ WCA875 resin is a flexible, non-reinforced extrudable blend of Polyphenylene Ether (PPE) + Thermoplastic Elastomer (TPE). This material contains non-halogenated flame retardant and performance capable of meeting UL VW-1 requirements, 105C end use temperature rating, and heat deformation performance as defined by UL 1581. FLEX NORYL WCA875 resin is intended for evaluation in wire insulation applications in dark colors. It has a Shore A Hardness reading of 87 and exhibits superior thermal stability, very low water absorption, good electric properties, and low specific gravity. Processing is typically conducted on standard extrusion equipment, and UL 1581 testing is conducted on 2.0mm wire with 0.12mm X 20 stranded copper conductor.

Diese Materialdaten wurden von Sabic zur Verfügung gestellt

Alle Daten beziehen sich auf Raumtemperatur soweit nicht anderweitig spezifiziert. SI Einheiten werden verwendt soweit nicht anderweitig spezifiziert.
Äquivalente Standards sind ähnlich zu einem oder mehreren Standards die der Anbieter angegeben hat. Manche äquivalente Standards können strikter sein oder außerhalb der Bedingungen des ursprünglichen Standards.

Ashby charts

Eigenschaften

Allgemein

PropertyTemperatureValueComment

Relative Dichte

23.0 °C

1.03 [-]

Show Supplier Material materials with Relative Dichte of 1.03 [-]

ASTM D 792 |

Sauerstoffindex

23.0 °C

29 %

Show Supplier Material materials with Sauerstoffindex of 29 %

Mechanisch

PropertyTemperatureValueComment

Biegemodul

23.0 °C

0 GPa

Show Supplier Material materials with Biegemodul of 0 GPa

ISO 178 | 12.5 mm/min

Dehnung

23.0 °C

170 %

Show Supplier Material materials with Dehnung of 170 %

ISO 527 | break, 50 mm/min

Härte, Shore A

23.0 °C

87 [-]

Show Supplier Material materials with Härte, Shore A of 87 [-]

ASTM D 2240 | 30S reading

Zugfestigkeit

23.0 °C

16 MPa

Show Supplier Material materials with Zugfestigkeit of 16 MPa

ISO 527 | break, 50 mm/min

Thermisch

PropertyValueComment

Brittleness temperature

-40 °C

Show Supplier Material materials with Brittleness temperature of -40 °C

<, ASTM D 746

Glow Wire Ignition Temperature

800 °C

Show Supplier Material materials with Glow Wire Ignition Temperature of 800 °C

IEC 60695-2-13 | 3.0 mm

Entflammbarkeit

Smoke Density on 0.5mm plaque, Flame, Ds, max: 146- ASTM E 662 <br> Glow Wire Flammability Index 960°C, passes at: 3mm IEC 60695-2-12 <br> Glow Wire Flammability Index 960°C, passes at: 3mm IEC 60695-2-12 <br> Smoke Density on 0.5mm plaque, Non-flame, Ds, max: 112- ASTM E 662

Elektrisch

PropertyTemperatureValueComment

Dielektrizitätskonstante, 1 MHz

23.0 °C

2.7 [-]

Show Supplier Material materials with Dielektrizitätskonstante, 1 MHz of 2.7 [-]

IEC 60250

Dissipation factor, 1MHz

23.0 °C

3.5E-3 [-]

Show Supplier Material materials with Dissipation factor, 1MHz of 3.5E-3 [-]

IEC 60250

Durchschlagfestigkeit

23.0 °C

22.8 kV/mm

Show Supplier Material materials with Durchschlagfestigkeit of 22.8 kV/mm

IEC 60243-1 | in oil, 2.0mm

Kriechstromfestigkeit

23.0 °C

600 V

Show Supplier Material materials with Kriechstromfestigkeit of 600 V

IEC 60112 |

Volume resistivity

23.0 °C

2.20E+0 - 1.00E+17 Ω·cm

Show Supplier Material materials with Volume resistivity of 2.20E+0 - 1.00E+17 Ω·cm

ASTM D 257

Rheological Properties

PropertyValueComment

Schmelzmassenflussrate

16 g/10min

Show Supplier Material materials with Schmelzmassenflussrate of 16 g/10min

ASTM D 1238 | 250°C/10.0 kgf

Technological properties

Property
Application areas

Medical Device, Data Transfer, Wire & cable

Availability

Europe,Asia,Americas

Processing methods

Feed Zone Temperature: 180 to 220.0°C
Melt Temperature: 220 to 250.0°C
Water Bath Temperature: 15 to 60.0°C
Screen Pack: 150 to 100.0-
Neck Temperature: 220 to 250.0°C
Maximum Moisture Content: 0.02%
Conductor Pre-heat Temperature: 25 to 120.0°C
Middle Zone Temperatures: 220 to 250.0°C
Die Temperature: 220 to 250.0°C
Screw Speed: 15 to 85.0rpm
Cross-head Temperature: 220 to 250.0°C
Cooling Water Air Gap: 100 to 200.0mm
Drying Temperature: 75 to 85.0°C
Head Zone Temperature: 220 to 250.0°C
Drying Time: 5 to 7.0hrs
Drying Time (Cumulative): 12hrs
Extruder Length/Diameter Ratio (L/D): 22:1 to 26:1-

Supplier Disclaimer

While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right.