Allgemein
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Biegefestigkeit | 23.0 °C | 105 MPa Show Supplier Material materials with Biegefestigkeit of 105 MPa | ASTM D 790 | brk, 1.3 mm/min, 50 mm span |
Biegemodul | 23.0 °C | 2.2 GPa Show Supplier Material materials with Biegemodul of 2.2 GPa | ASTM D 790 | 1.3 mm/min, 50 mm span |
Dehnung | 23.0 °C | 7.5 % Show Supplier Material materials with Dehnung of 7.5 % | ASTM D 638 | yld, Type I, 50 mm/min |
Elastizitätsmodul | 23.0 °C | 2.2 GPa Show Supplier Material materials with Elastizitätsmodul of 2.2 GPa | ASTM D 638 | 50 mm/min |
Impact strength, Izod notched, ASTM | 23.0 °C | 578 J/m Show Supplier Material materials with Impact strength, Izod notched, ASTM of 578 J/m | ASTM D 256 | notched, 23°C |
Impact strength, Izod unnotched, ASTM | 23.0 °C | 2140 J/m Show Supplier Material materials with Impact strength, Izod unnotched, ASTM of 2140 J/m | ASTM D 4812 | 23°C |
Instrumented Impact, Total Energy | 23.0 °C | 77 J Show Supplier Material materials with Instrumented Impact, Total Energy of 77 J | ASTM D 3763 | 23°C |
Instrumented Impact, at Peak | 23.0 °C | 73 J Show Supplier Material materials with Instrumented Impact, at Peak of 73 J | ASTM D 3763 | 23°C |
Schlagzähigkeit, Izod gekerbt | 23.0 °C | 578 kJ/m² Show Supplier Material materials with Schlagzähigkeit, Izod gekerbt of 578 kJ/m² | ASTM D 256 | notched, 23°C |
Zugfestigkeit | 23.0 °C | 68 MPa Show Supplier Material materials with Zugfestigkeit of 68 MPa | ASTM D 638 | yld, Type I, 50 mm/min |
Thermisch
Property | Value | Comment |
---|---|---|
Ball Pressure Test | PASS | IEC 60695-10-2 | 125°C +/- 2°C |
Heat deflection temperature, 0.45 MPa | 160 °C Show Supplier Material materials with Heat deflection temperature, 0.45 MPa of 160 °C | ASTM D 648 | 3.2 mm, unannealed |
Heat deflection temperature, 1.80 MPa | 147 °C Show Supplier Material materials with Heat deflection temperature, 1.80 MPa of 147 °C | ASTM D 648 | 3.2mm, unannealed |
Vicat-Erweichungstemperatur | 164 °C Show Supplier Material materials with Vicat-Erweichungstemperatur of 164 °C | ASTM D 1525 | Rate B/50 |
Wärmeformbeständigkeitstemperatur | 147 - 160 °C Show Supplier Material materials with Wärmeformbeständigkeitstemperatur of 147 - 160 °C |
Rheological Properties
Property | Value | Comment |
---|---|---|
Schmelzmassenflussrate | 15 g/10min Show Supplier Material materials with Schmelzmassenflussrate of 15 g/10min | ASTM D 1238 | 330°C/2.16 kgf |
Technological properties
Property | ||
---|---|---|
Application areas | Enclosures | |
Availability | Europe,Americas | |
Processing methods | Melt Temperature: 350 to 370.0°C | |
Supplier Disclaimer | While the information is provided in good faith, SABIC MAKES NO WARRANTY, EXPRESS OR IMPLIED, INCLUDING MERCHANTABILITY AND NONINFRINGEMENT OF INTELLECTUAL PROPERTY, NOR ASSUMES ANY LIABILITY, DIRECT OR INDIRECT, WITH RESPECT TO THE PERFORMANCE, SUITABILITY OR FITNESS FOR INTENDED USE OR PURPOSE OF THESE PRODUCTS IN ANY APPLICATION. Each Buyer must determine the suitability of SABIC's materials for the Buyer's particular use through appropriate testing and analysis. No statement by SABIC concerning a possible use of any product, service or design is intended, or should be construed, to grant any license under any patent or other intellectual property right. |