Allgemein
Property | Temperature | Value |
---|---|---|
Dichte | 23.0 °C | 8.1 g/cm³ Show Supplier Material materials with Dichte of 8.1 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Härte, Rockwell B | 23.0 °C | 90 [-] Show Supplier Material materials with Härte, Rockwell B of 90 [-] | max. |
Streckgrenze Rp 0,2 | 20.0 °C | 241 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 241 MPa | min. |
100.0 °C | 220 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 220 MPa | min. | |
150.0 °C | 210 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 210 MPa | min. | |
200.0 °C | 201 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 201 MPa | min. | |
250.0 °C | 193 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 193 MPa | min. | |
300.0 °C | 186 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 186 MPa | min. | |
350.0 °C | 181 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 181 MPa | min. | |
400.0 °C | 177 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 177 MPa | min. | |
450.0 °C | 175 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 175 MPa | min. | |
500.0 °C | 174 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 174 MPa | min. | |
525.0 °C | 172 MPa Show Supplier Material materials with Streckgrenze Rp 0,2 of 172 MPa | min. | |
Verlängerung A2 | 23.0 °C | 30 % Show Supplier Material materials with Verlängerung A2 of 30 % | min. |
Zugfestigkeit | 23.0 °C | 586 MPa Show Supplier Material materials with Zugfestigkeit of 586 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 1.42E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.42E-5 1/K | for 30°C to the mentioned temperature |
200.0 °C | 1.46E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.46E-5 1/K | for 30°C to the mentioned temperature | |
300.0 °C | 1.49E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.49E-5 1/K | for 30°C to the mentioned temperature | |
400.0 °C | 1.51E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.51E-5 1/K | for 30°C to the mentioned temperature | |
500.0 °C | 1.53E-5 1/K Show Supplier Material materials with Koeffizient der thermischen Ausdehnung of 1.53E-5 1/K | for 30°C to the mentioned temperature | |
Spezifische Wärmekapazität | 20.0 °C | 440 J/(kg·K) Show Supplier Material materials with Spezifische Wärmekapazität of 440 J/(kg·K) | |
Wärmeleitfähigkeit | 20.0 °C | 11 W/(m·K) Show Supplier Material materials with Wärmeleitfähigkeit of 11 W/(m·K) |
Chemical properties
Property | Value | Comment | |
---|---|---|---|
Chrom | 20 % Show Supplier Material materials with Chrom of 20 % | ||
Eisen | Balance | ||
Kohlenstoff | 0.03 % Show Supplier Material materials with Kohlenstoff of 0.03 % | max. | |
Kupfer | 1.7 % Show Supplier Material materials with Kupfer of 1.7 % | ||
Mangan | 0.8 % Show Supplier Material materials with Mangan of 0.8 % | ||
Molybdän | 2.6 % Show Supplier Material materials with Molybdän of 2.6 % | ||
Nickel | 38.5 % Show Supplier Material materials with Nickel of 38.5 % | ||
Phosphor | 0.03 % Show Supplier Material materials with Phosphor of 0.03 % | max. | |
Schwefel | 0.01 % Show Supplier Material materials with Schwefel of 0.01 % | max. | |
Silizium | 0.5 % Show Supplier Material materials with Silizium of 0.5 % | max. | |
Titan | 0.7 % Show Supplier Material materials with Titan of 0.7 % |
Technological properties
Property | ||
---|---|---|
Application areas | Sanicro® 41 is particularly suited for use in heat exchangers for crude oil and oil refineries, especially where high concentrations of hydrogen sulphide and chloride are present. | |
Certifications | Approvals: | |
Cold Forming | The excellent formability of Sanicro® 41 enables the material to be cold bent to extremely small radii. Annealing after bending is not normally necessary. | |
Corrosion properties | General corrosion: Sanicro® 41 possesses excellent resistance to corrosion. The material is far superior to molybdenum alloyed steels such as AISI 316L, particularly when exposed to non-oxidizing media such as sulfuric acid or phosphoric acid. It also has satisfactory resistance to highly oxidizing agents such as nitric acid. Sanicro® 41 has significantly better corrosion resistance in formic acid than standard austenitic stainless steels. The results of corrosion tests in nitric acid are tabulated below. Resistance to sulfuric acid is illustrated in Figure 1. It should be noted that the corrosiveness of sulfuric acid depends on the oxygen content. Sulfuric acid in contact with air is, therefore, more corrosive than deaerated acid. Pitting and crevice corrosion:Corrosion tests carried out in sodium chloride solutions indicate that the resistance of Sanicro® 41 to pitting and crevice corrosion is superior to that of AISI 316- a result of the higher chromium and molybdenum contents of the material. Critical pitting temperatures (CPT) for the two grades in 3% sodium chloride solutions at different pH values are plotted in Figure 2. Stress corrosion cracking:The high nickel content of the material promotes excellent resistance to stress corrosion cracking induced by both chlorides and alkalis. The results of stress corrosion cracking tests in 40 % calcium chloride are shown in Figure 3. Sanicro® 41 displays excellent resistance to stress corrosion cracking in sour environments. Tests carried out at the Nickel Development Institute (NIDI), concluded that Sanicro® 41 could be used in sour environments up to 260°C with H₂S contents corresponding to a partial pressure of up to 10000 psi, in the absence of elementary sulfur. The material also shows some immunity to all concentrations of CO2, according to NIDI. Sanicro 41 is used in the oil and gas industry in environments up to 200°C (392°F), a 60 psi partial pressure of H₂S and with chlorides present. According to ISO 15156/NACE MR0175 it is acceptable for use in the cold worked and annealed condition with no environmental limits in respect of partial pressures of H₂S or elemental sulfur. Intergranular corrosion: Even in the heaviest sizes, Sanicro® 41 can be welded without the risk of carbide precipitation causing intergranular corrosion. This is due, in part, to the low carbon content of the material, but also to the fact that it is titanium stabilized. | |
Heat Treatment | Tubes are delivered in the heat treated condition. If additional heat treatment is needed due to further processing, the following is recommended. Solution annealing: 1000-1100°C (1830-2010°F), 5-10 minutes, rapid cooling in air or water. | |
Other | Forms of supply: Seamless tube and pipe- finishes and dimensions: Heat exchanger tubing, straight or bent to specification, with or without heat treatment of bends, can be supplied. Seamless tube and pipe in Sanicro® 41 can be supplied in dimensions up to 260 mm (10") outside diameter. The delivery condition is solution annealed and either white pickled or bright annealed. Materials for oil and gas production Cold worked seamless tube and pipe: Size range: | |
Welding | The weldability of Sanicro® 41 is good. Suitable methods of fusion welding are manual metal-arc welding (MMA/SMAW) and gas-shielded arc welding, with the TIG/GTAW method as first choice. Since the material has low thermal conductivity and high thermal expansion. Welding plans should therefore be carefully selected in advance, so that distortions of the welded joint are minimized. If residual stresses are a concern, solution annealing can be performed after welding. For Sanicro® 41, heat-input of <1.0 kJ/mm and interpass temperature of <100°C (210°F) are recommended. A string bead welding technique should be used. Recommended filler metals for temperature
Overlay welding: |