Mechanisch
Property | Temperature | Value |
---|---|---|
Dehnung A50 | 20.0 °C | 20 % Show Material materials with Dehnung A50 of 20 % |
316.0 °C | 25 % Show Material materials with Dehnung A50 of 25 % | |
Dehnung A50, transversal | 20.0 °C | 20 % Show Material materials with Dehnung A50, transversal of 20 % |
316.0 °C | 30 % Show Material materials with Dehnung A50, transversal of 30 % | |
Streckgrenze Rp 0,2 | 20.0 °C | 151 MPa Show Material materials with Streckgrenze Rp 0,2 of 151 MPa |
316.0 °C | 76 MPa Show Material materials with Streckgrenze Rp 0,2 of 76 MPa | |
Streckgrenze Rp 0,2, transversal | 20.0 °C | 172 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 172 MPa |
316.0 °C | 96 MPa Show Material materials with Streckgrenze Rp 0,2, transversal of 96 MPa | |
Zugfestigkeit | 20.0 °C | 400 MPa Show Material materials with Zugfestigkeit of 400 MPa |
316.0 °C | 172 MPa Show Material materials with Zugfestigkeit of 172 MPa | |
Zugfestigkeit, transversal | 20.0 °C | 310 MPa Show Material materials with Zugfestigkeit, transversal of 310 MPa |
316.0 °C | 158 MPa Show Material materials with Zugfestigkeit, transversal of 158 MPa | |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.01 % Show Material materials with Aluminium of 0.01 % |
Chrom | 0.01 % Show Material materials with Chrom of 0.01 % |
Eisen | 0.05 % Show Material materials with Eisen of 0.05 % |
Kohlenstoff | 0.015 % Show Material materials with Kohlenstoff of 0.015 % |
Kupfer | 0.01 % Show Material materials with Kupfer of 0.01 % |
Molybdän | 2E-3 % Show Material materials with Molybdän of 2E-3 % |
Nickel | 5E-3 % Show Material materials with Nickel of 5E-3 % |
Niobium | 0.01 % Show Material materials with Niobium of 0.01 % |
Sauerstoff | 0.04 % Show Material materials with Sauerstoff of 0.04 % |
Silizium | 0.01 % Show Material materials with Silizium of 0.01 % |
Stickstoff | 0.01 % Show Material materials with Stickstoff of 0.01 % |
Tantal | 0.02 % Show Material materials with Tantal of 0.02 % |
Titan | 0.01 % Show Material materials with Titan of 0.01 % |
Uran | 1E-3 % Show Material materials with Uran of 1E-3 % |
Vanadium | 5E-3 % Show Material materials with Vanadium of 5E-3 % |
Wasserstoff | 2.5E-3 % Show Material materials with Wasserstoff of 2.5E-3 % |
Wolfram | 0.02 % Show Material materials with Wolfram of 0.02 % |
Zinn | 5E-3 % Show Material materials with Zinn of 5E-3 % |