Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20.0 °C | 2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Flat | A100 |
20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | A10 | |
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | ||
Elastizitätsmodul | 20.0 °C | 60.0 - 65.0 GPa Show Material materials with Elastizitätsmodul of 60.0 - 65.0 GPa | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | |
Härte, Brinell | 20.0 °C | 47.0 [-] Show Material materials with Härte, Brinell of 47.0 [-] | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||||
Schubmodule | 20.0 °C | 24.0 - 26.0 GPa Show Material materials with Schubmodule of 24.0 - 26.0 GPa | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | |
Zugfestigkeit | 20.0 °C | 160.0 MPa Show Material materials with Zugfestigkeit of 160.0 MPa | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | |
20.0 °C | 160.0 - 200.0 MPa Show Material materials with Zugfestigkeit of 160.0 - 200.0 MPa | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50.0 °C | 2.17e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | |
100.0 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | ||
200.0 °C | 2.44e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.44e-05 1/K | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | ||
300.0 °C | 2.54e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.54e-05 1/K | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | ||
Schmelzpunkt | 645.0 - 660.0 °C Show Material materials with Schmelzpunkt of 645.0 - 660.0 °C | Typical for Wrought 1000 Series Aluminium | ||||
Spezifische Wärmekapazität | 900.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 - 963.0 J/(kg·K) | Typical for Wrought 1000 Series Aluminium | ||||
Wärmeleitfähigkeit | 20.0 °C | 205.0 - 210.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 205.0 - 210.0 W/(m·K) | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 34400000.0 - 35500000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 34400000.0 - 35500000.0 S/m | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | |
spezifischer Widerstand | 2.7e-08 - 3e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.7e-08 - 3e-08 Ω·m | Typical for Wrought 1000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Kupfer | 0.05 Show Material materials with Kupfer of 0.05 | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip |
Magnesium | 0.05 Show Material materials with Magnesium of 0.05 | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip |
Mangan | 0.05 Show Material materials with Mangan of 0.05 | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip |
Titan | 0.05 Show Material materials with Titan of 0.05 | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip |
Zink | 0.1 Show Material materials with Zink of 0.1 | H1x | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent | |
Workability | Excellent workability. |