Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
20.0 °C | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 25.0 MPa Show Material materials with Bending Fatigue Strength of 25.0 MPa | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | |||
Biegewinkel 180° | 0.5 °/t Show Material materials with Biegewinkel 180° of 0.5 °/t | O | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Biegewinkel 180° of 1.0 °/t | O | EN 573-3, EN 485 | ||||
Biegewinkel 90° | 0.5 °/t Show Material materials with Biegewinkel 90° of 0.5 °/t | O | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | O | EN 573-3, EN 485 | ||||
Dehnung | 1.0 % Show Material materials with Dehnung of 1.0 % | O | EN 573-3, EN 546 | A50 | ||
2.0 % Show Material materials with Dehnung of 2.0 % | O | EN 573-3, EN 546 | A50 | |||
4.0 % Show Material materials with Dehnung of 4.0 % | O | EN 573-3, EN 546 | A50 | |||
6.0 % Show Material materials with Dehnung of 6.0 % | O | EN 573-3, EN 546, EN 683 | A50 | |||
10.0 % Show Material materials with Dehnung of 10.0 % | O | EN 573-3, EN 546, EN 683 | A50 | |||
15.0 % Show Material materials with Dehnung of 15.0 % | O | EN 573-3, EN 683 | A50 | |||
20.0 % Show Material materials with Dehnung of 20.0 % | O | EN 573-3, EN 1396, EN 485 | A50 | |||
22.0 % Show Material materials with Dehnung of 22.0 % | O | EN 573-3, EN 1396, EN 485, EN 754 | A50 | |||
23.0 % Show Material materials with Dehnung of 23.0 % | O | EN 573-3, EN 755 | A50 | |||
25.0 % Show Material materials with Dehnung of 25.0 % | O | EN 573-3, EN 754, EN 755 | A100 | |||
26.0 % Show Material materials with Dehnung of 26.0 % | O | EN 573-3, EN 1396, EN 485 | A50 | |||
29.0 % Show Material materials with Dehnung of 29.0 % | O | EN 573-3, EN 485 | A50 | |||
32.0 % Show Material materials with Dehnung of 32.0 % | O | EN 573-3, EN 485 | A100 | |||
35.0 % Show Material materials with Dehnung of 35.0 % | O | EN 573-3, EN 1301 | ||||
35.0 % Show Material materials with Dehnung of 35.0 % | O | EN 573-3, EN 485 | A50 | |||
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Flat | A100 | |
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Flat | A100 | |
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Flat | A100 | |
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Flat | A100 | |
20.0 °C | 18.0 % Show Material materials with Dehnung of 18.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire | A100 | |
20.0 °C | 22.0 % Show Material materials with Dehnung of 22.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire | A10 | |
20.0 °C | 23.0 % Show Material materials with Dehnung of 23.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Tube | A10 | |
20.0 °C | 27.0 % Show Material materials with Dehnung of 27.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Tube | ||
20.0 °C | 30.0 % Show Material materials with Dehnung of 30.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Flat | A10 | |
20.0 °C | 35.0 % Show Material materials with Dehnung of 35.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | A10 | |
20.0 °C | 35.0 % Show Material materials with Dehnung of 35.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Sheet | ||
20.0 °C | 40.0 % Show Material materials with Dehnung of 40.0 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Strip, Sheet | ||
Elastizitätsmodul | -195.0 °C | 78.4 GPa Show Material materials with Elastizitätsmodul of 78.4 GPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
-85.0 °C | 73.5 GPa Show Material materials with Elastizitätsmodul of 73.5 GPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
-30.0 °C | 71.4 GPa Show Material materials with Elastizitätsmodul of 71.4 GPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | ||||
20.0 °C | 60.0 - 70.0 GPa Show Material materials with Elastizitätsmodul of 60.0 - 70.0 GPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
100.0 °C | 68.6 GPa Show Material materials with Elastizitätsmodul of 68.6 GPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
150.0 °C | 66.5 GPa Show Material materials with Elastizitätsmodul of 66.5 GPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
200.0 °C | 63.0 GPa Show Material materials with Elastizitätsmodul of 63.0 GPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
250.0 °C | 56.0 GPa Show Material materials with Elastizitätsmodul of 56.0 GPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
Härte, Brinell | 20.0 [-] Show Material materials with Härte, Brinell of 20.0 [-] | O | EN 573-3, EN 485 | |||
20.0 °C | 20.0 [-] Show Material materials with Härte, Brinell of 20.0 [-] | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Strip, Tube, Wire, Sheet | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||||
Schubmodule | 25.9 GPa Show Material materials with Schubmodule of 25.9 GPa | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | |||
20.0 °C | 25.0 - 26.5 GPa Show Material materials with Schubmodule of 25.0 - 26.5 GPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
Zugfestigkeit | 35.0 - 80.0 MPa Show Material materials with Zugfestigkeit of 35.0 - 80.0 MPa | O | EN 573-3, EN 546 | |||
40.0 - 85.0 MPa Show Material materials with Zugfestigkeit of 40.0 - 85.0 MPa | O | EN 573-3, EN 546 | ||||
45.0 - 95.0 MPa Show Material materials with Zugfestigkeit of 45.0 - 95.0 MPa | O | EN 573-3, EN 546 | ||||
45.0 - 90.0 MPa Show Material materials with Zugfestigkeit of 45.0 - 90.0 MPa | O | EN 573-3, EN 546 | ||||
50.0 - 95.0 MPa Show Material materials with Zugfestigkeit of 50.0 - 95.0 MPa | O | EN 573-3, EN 546, EN 683 | ||||
60.0 - 80.0 MPa Show Material materials with Zugfestigkeit of 60.0 - 80.0 MPa | O | EN 573-3, EN 1715-3 | ||||
60.0 MPa Show Material materials with Zugfestigkeit of 60.0 MPa | O | EN 573-3, EN 755 | ||||
95.0 MPa Show Material materials with Zugfestigkeit of 95.0 MPa | O | EN 573-3, EN 1301 | ||||
20.0 °C | 55.0 - 90.0 MPa Show Material materials with Zugfestigkeit of 55.0 - 90.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Flat | ||
20.0 °C | 55.0 - 95.0 MPa Show Material materials with Zugfestigkeit of 55.0 - 95.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Flat | ||
20.0 °C | 60.0 MPa Show Material materials with Zugfestigkeit of 60.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Wire | ||
20.0 °C | 60.0 - 90.0 MPa Show Material materials with Zugfestigkeit of 60.0 - 90.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Flat | ||
20.0 °C | 60.0 - 95.0 MPa Show Material materials with Zugfestigkeit of 60.0 - 95.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4, EN 754, EN 755 | Flat | ||
20.0 °C | 65.0 MPa Show Material materials with Zugfestigkeit of 65.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Tube | ||
20.0 °C | 65.0 - 95.0 MPa Show Material materials with Zugfestigkeit of 65.0 - 95.0 MPa | O | DIN 1712-3, EN 573-3, EN 573-4, EN 1396, EN 485 | Strip, Sheet, Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.17e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755, DIN 1712-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire |
-50.0 °C | 2.17e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755, DIN 1712-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
20 °C | 2.17e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755, DIN 1712-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
20 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755, DIN 1712-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
20 °C | 2.4399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4399999999999997e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
20 °C | 2.5399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5399999999999997e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
100 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755, DIN 1712-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
100.0 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755, DIN 1712-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
200 °C | 2.4399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4399999999999997e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
200.0 °C | 2.44e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.44e-05 1/K | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
300 °C | 2.5399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5399999999999997e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
300.0 °C | 2.54e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.54e-05 1/K | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
Schmelzpunkt | 646.0 - 657.0 °C Show Material materials with Schmelzpunkt of 646.0 - 657.0 °C | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
Wärmeleitfähigkeit | 20.0 °C | 210.0 - 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 210.0 - 220.0 W/(m·K) | O | DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Rod, Sheet, Flat, Strip, Tube, Wire |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 34000000.0 - 36000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 34000000.0 - 36000000.0 S/m | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
20.0 °C | 34800000.0 - 36000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 34800000.0 - 36000000.0 S/m | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
spezifischer Widerstand | 2.78e-08 - 2.94e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.78e-08 - 2.94e-08 Ω·m | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 99.5 % Show Material materials with Aluminium of 99.5 % | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | |
Eisen | 0.4 % Show Material materials with Eisen of 0.4 % | O | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire |
0.40 % Show Material materials with Eisen of 0.40 % | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | O | DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Rod, Sheet, Flat, Strip, Tube, Wire |
Magnesium | 0.05 % Show Material materials with Magnesium of 0.05 % | O | DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Rod, Sheet, Flat, Strip, Tube, Wire |
Mangan | 0.05 % Show Material materials with Mangan of 0.05 % | O | DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Rod, Sheet, Flat, Strip, Tube, Wire |
Silizium | 0.25 % Show Material materials with Silizium of 0.25 % | O | DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Rod, Sheet, Flat, Strip, Tube, Wire |
Titan | 0.05 % Show Material materials with Titan of 0.05 % | O | DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Rod, Sheet, Flat, Strip, Tube, Wire |
Zink | 0.07 % Show Material materials with Zink of 0.07 % | O | DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Rod, Sheet, Flat, Strip, Tube, Wire |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: gut (EQ: sehr gut), Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: acceptable, weathering: good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H14) / very good (H12) |