Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.73 g/cm³ Show Material materials with Dichte of 2.73 g/cm³ | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
20.0 °C | 2.73 g/cm³ Show Material materials with Dichte of 2.73 g/cm³ | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 50.0 MPa Show Material materials with Bending Fatigue Strength of 50.0 MPa | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | |||
Biegewinkel 180° | 1.0 °/t Show Material materials with Biegewinkel 180° of 1.0 °/t | O | EN 573-3, EN 485 | |||
Biegewinkel 90° | 1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | O | EN 573-3, EN 485 | |||
1.5 °/t Show Material materials with Biegewinkel 90° of 1.5 °/t | O | EN 573-3, EN 485 | ||||
Dehnung | -196.0 °C | 46.0 % Show Material materials with Dehnung of 46.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | ||
-80.0 °C | 42.0 % Show Material materials with Dehnung of 42.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
-28.0 °C | 41.0 % Show Material materials with Dehnung of 41.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
7.0 % Show Material materials with Dehnung of 7.0 % | O | EN 573-3, EN 546 | A50 | |||
8.0 % Show Material materials with Dehnung of 8.0 % | O | EN 573-3, EN 546 | A50 | |||
10.0 % Show Material materials with Dehnung of 10.0 % | O | EN 573-3, EN 683 | A50 | |||
12.0 % Show Material materials with Dehnung of 12.0 % | O | EN 573-3, EN 546 | A50 | |||
13.0 % Show Material materials with Dehnung of 13.0 % | O | EN 573-3, EN 683 | A50 | |||
15.0 % Show Material materials with Dehnung of 15.0 % | O | EN 573-3, EN 485, EN 546, EN 683 | A50 | |||
16.0 % Show Material materials with Dehnung of 16.0 % | O | EN 573-3, EN 754 | A50 | |||
17.0 % Show Material materials with Dehnung of 17.0 % | O | EN 573-3, EN 485 | A50 | |||
20.0 % Show Material materials with Dehnung of 20.0 % | O | EN 573-3, EN 485, EN 754, EN 755 | A50 | |||
23.0 % Show Material materials with Dehnung of 23.0 % | O | EN 573-3, EN 485 | A100 | |||
23.0 % Show Material materials with Dehnung of 23.0 % | O | EN 573-3, EN 485 | A50 | |||
24.0 % Show Material materials with Dehnung of 24.0 % | O | EN 573-3, EN 485 | A50 | |||
25.0 % Show Material materials with Dehnung of 25.0 % | O | EN 573-3, EN 754, EN 755 | A100 | |||
35.0 % Show Material materials with Dehnung of 35.0 % | O | EN 573-3, EN 1301 | ||||
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat | A100 | |
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat | A100 | |
20.0 °C | 18.0 % Show Material materials with Dehnung of 18.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat | A100 | |
20.0 °C | 25.0 % Show Material materials with Dehnung of 25.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip | A10 | |
20.0 °C | 28.0 % Show Material materials with Dehnung of 28.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
20.0 °C | 40.0 % Show Material materials with Dehnung of 40.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
100.0 °C | 43.0 % Show Material materials with Dehnung of 43.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
150.0 °C | 47.0 % Show Material materials with Dehnung of 47.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
200.0 °C | 60.0 % Show Material materials with Dehnung of 60.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
260.0 °C | 65.0 % Show Material materials with Dehnung of 65.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
315.0 °C | 70.0 % Show Material materials with Dehnung of 70.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
370.0 °C | 70.0 % Show Material materials with Dehnung of 70.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | |||
69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | ||||
20.0 °C | 65.0 GPa Show Material materials with Elastizitätsmodul of 65.0 GPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip | ||
Härte, Brinell | 28.0 [-] Show Material materials with Härte, Brinell of 28.0 [-] | O | EN 573-3, EN 485 | |||
20.0 °C | 30.0 [-] Show Material materials with Härte, Brinell of 30.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||||
Schubmodule | 26.1 GPa Show Material materials with Schubmodule of 26.1 GPa | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | |||
20.0 °C | 26.5 GPa Show Material materials with Schubmodule of 26.5 GPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip | ||
Zugfestigkeit | -196.0 °C | 230.0 MPa Show Material materials with Zugfestigkeit of 230.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | ||
-80.0 °C | 140.0 MPa Show Material materials with Zugfestigkeit of 140.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
-28.0 °C | 120.0 MPa Show Material materials with Zugfestigkeit of 120.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
85.0 - 135.0 MPa Show Material materials with Zugfestigkeit of 85.0 - 135.0 MPa | O | EN 573-3, EN 546, EN 683 | ||||
95.0 - 135.0 MPa Show Material materials with Zugfestigkeit of 95.0 - 135.0 MPa | O | EN 573-3, EN 485, EN 755 | ||||
95.0 - 130.0 MPa Show Material materials with Zugfestigkeit of 95.0 - 130.0 MPa | O | EN 573-3, EN 754 | ||||
130.0 MPa Show Material materials with Zugfestigkeit of 130.0 MPa | O | EN 573-3, EN 1301 | ||||
20.0 °C | 100.0 - 145.0 MPa Show Material materials with Zugfestigkeit of 100.0 - 145.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
20.0 °C | 100.0 - 140.0 MPa Show Material materials with Zugfestigkeit of 100.0 - 140.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
20.0 °C | 110.0 MPa Show Material materials with Zugfestigkeit of 110.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
100.0 °C | 90.0 MPa Show Material materials with Zugfestigkeit of 90.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
150.0 °C | 75.0 MPa Show Material materials with Zugfestigkeit of 75.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
200.0 °C | 60.0 MPa Show Material materials with Zugfestigkeit of 60.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
260.0 °C | 40.0 MPa Show Material materials with Zugfestigkeit of 40.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
315.0 °C | 30.0 MPa Show Material materials with Zugfestigkeit of 30.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | |||
370.0 °C | 20.0 MPa Show Material materials with Zugfestigkeit of 20.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.1499999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1499999999999997e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | |
-50.0 °C | 2.15e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.15e-05 1/K | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip | |
20 °C | 2.1499999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1499999999999997e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3199999999999998e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
20 °C | 2.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.41e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755, DIN 1725-1, EN 573-4 | Sheet, Flat, Strip | |
20 °C | 2.52e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.52e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755, DIN 1725-1, EN 573-4 | Sheet, Flat, Strip | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3199999999999998e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
100.0 °C | 2.32e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.32e-05 1/K | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip | |
200 °C | 2.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.41e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755, DIN 1725-1, EN 573-4 | Sheet, Flat, Strip | |
200.0 °C | 2.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.41e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755, DIN 1725-1, EN 573-4 | Sheet, Flat, Strip | |
300 °C | 2.52e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.52e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755, DIN 1725-1, EN 573-4 | Sheet, Flat, Strip | |
300.0 °C | 2.52e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.52e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755, DIN 1725-1, EN 573-4 | Sheet, Flat, Strip | |
Schmelzpunkt | 640.0 - 655.0 °C Show Material materials with Schmelzpunkt of 640.0 - 655.0 °C | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
643.0 - 654.0 °C Show Material materials with Schmelzpunkt of 643.0 - 654.0 °C | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | |||
Spezifische Wärmekapazität | 893.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 893.0 J/(kg·K) | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
20.0 °C | 893.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 893.0 J/(kg·K) | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip | |
Wärmeleitfähigkeit | 159.0 - 193.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 159.0 - 193.0 W/(m·K) | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
20.0 °C | 160.0 - 200.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 - 200.0 W/(m·K) | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Sheet, Flat, Strip |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 24000000.0 - 29000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 24000000.0 - 29000000.0 S/m | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
20.0 °C | 23000000.0 - 29000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 29000000.0 S/m | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Sheet, Flat, Strip | |
spezifischer Widerstand | 3.45e-08 - 4.17e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.45e-08 - 4.17e-08 Ω·m | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
3.45e-08 - 4.35e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.45e-08 - 4.35e-08 Ω·m | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Eisen | 0.7 % Show Material materials with Eisen of 0.7 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip |
0.70 % Show Material materials with Eisen of 0.70 % | O | EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | ||
Kupfer | 0.05 - 0.2 % Show Material materials with Kupfer of 0.05 - 0.2 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Sheet, Flat, Strip |
Mangan | 1.0 - 1.5 % Show Material materials with Mangan of 1.0 - 1.5 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Sheet, Flat, Strip |
Silizium | 0.6 % Show Material materials with Silizium of 0.6 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Sheet, Flat, Strip |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | O | DIN 1725-1, EN 573-3, EN 573-4, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755 | Sheet, Flat, Strip |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (O) / very good (H12) |