Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20.0 °C | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Wire | A100 |
20.0 °C | 20.0 % Show Material materials with Dehnung of 20.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire | A10 | |
20.0 °C | 23.0 % Show Material materials with Dehnung of 23.0 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Elastizitätsmodul | 20.0 °C | 70.0 Show Material materials with Elastizitätsmodul of 70.0 | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire | |
Härte, Brinell | 20.0 °C | 23.0 [-] Show Material materials with Härte, Brinell of 23.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Schubmodule | 20.0 °C | 27.0 Show Material materials with Schubmodule of 27.0 | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire | |
Zugfestigkeit | 20.0 °C | 70.0 MPa Show Material materials with Zugfestigkeit of 70.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Wire | |
20.0 °C | 80.0 - 120.0 MPa Show Material materials with Zugfestigkeit of 80.0 - 120.0 MPa | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.2e-05 - 2.5e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 - 2.5e-05 1/K | Typical for Wrought 5000 Series Aluminium | ||||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 560.0 - 655.0 °C Show Material materials with Schmelzpunkt of 560.0 - 655.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Spezifische Wärmekapazität | 879.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium | ||||
Wärmeleitfähigkeit | 20.0 °C | 215.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 215.0 W/(m·K) | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 35000000.0 Show Material materials with Elektrische Leitfähigkeit of 35000000.0 | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire | |
spezifischer Widerstand | 3.3e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.3e-08 - 5e-08 Ω·m | Typical for Wrought 5000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Eisen | 0.08 Show Material materials with Eisen of 0.08 | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire |
Magnesium | 0.3 - 0.6 % Show Material materials with Magnesium of 0.3 - 0.6 % | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire |
Mangan | 0.03 Show Material materials with Mangan of 0.03 | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire |
Silizium | 0.08 Show Material materials with Silizium of 0.08 | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire |
Titan | 0.02 Show Material materials with Titan of 0.02 | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire |
Zink | 0.05 Show Material materials with Zink of 0.05 | O | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip, Wire |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |