Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20.0 °C | 2.64 g/cm³ Show Material materials with Dichte of 2.64 g/cm³ | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging, Profile, Rod, Tube |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging | |
20.0 °C | 11.0 % Show Material materials with Dehnung of 11.0 % | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Profile, Rod, Tube | A10 | |
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging | ||
20.0 °C | 13.0 % Show Material materials with Dehnung of 13.0 % | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Profile, Rod, Tube | ||
Elastizitätsmodul | 20.0 °C | 67.0 - 72.0 GPa Show Material materials with Elastizitätsmodul of 67.0 - 72.0 GPa | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging, Profile, Rod, Tube | |
Härte, Brinell | 20.0 °C | 55.0 [-] Show Material materials with Härte, Brinell of 55.0 [-] | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging, Profile | |
20.0 °C | 60.0 [-] Show Material materials with Härte, Brinell of 60.0 [-] | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Rod | ||
20.0 °C | 65.0 [-] Show Material materials with Härte, Brinell of 65.0 [-] | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Schubmodule | 20.0 °C | 27.0 GPa Show Material materials with Schubmodule of 27.0 GPa | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging, Profile, Rod, Tube | |
Zugfestigkeit | 20.0 °C | 240.0 MPa Show Material materials with Zugfestigkeit of 240.0 MPa | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging | |
20.0 °C | 250.0 MPa Show Material materials with Zugfestigkeit of 250.0 MPa | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Profile, Rod, Tube | ||
20.0 °C | 260.0 MPa Show Material materials with Zugfestigkeit of 260.0 MPa | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50.0 °C | 2.25e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.25e-05 1/K | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging, Profile, Rod, Tube | |
100.0 °C | 2.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.41e-05 1/K | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging, Profile, Rod, Tube | ||
200.0 °C | 2.51e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.51e-05 1/K | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging, Profile, Rod, Tube | ||
300.0 °C | 2.61e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.61e-05 1/K | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging, Profile, Rod, Tube | ||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 560.0 - 655.0 °C Show Material materials with Schmelzpunkt of 560.0 - 655.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Spezifische Wärmekapazität | 20.0 °C | 904.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 904.0 J/(kg·K) | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging, Profile, Rod, Tube | |
Wärmeleitfähigkeit | 20.0 °C | 110.0 - 140.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 110.0 - 140.0 W/(m·K) | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging, Profile, Rod, Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 15000000.0 - 19000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 15000000.0 - 19000000.0 S/m | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging, Profile, Rod, Tube | |
spezifischer Widerstand | 3.3e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.3e-08 - 5e-08 Ω·m | Typical for Wrought 5000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.2 Show Material materials with Chrom of 0.2 | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging, Profile, Rod, Tube |
Eisen | 0.5 Show Material materials with Eisen of 0.5 | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging, Profile, Rod, Tube |
Kupfer | 0.1 Show Material materials with Kupfer of 0.1 | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging, Profile, Rod, Tube |
Magnesium | 4.5 - 5.6 % Show Material materials with Magnesium of 4.5 - 5.6 % | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging, Profile, Rod, Tube |
Mangan | 0.1 - 0.6 % Show Material materials with Mangan of 0.1 - 0.6 % | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging, Profile, Rod, Tube |
Silizium | 0.4 Show Material materials with Silizium of 0.4 | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging, Profile, Rod, Tube |
Titan | 0.2 Show Material materials with Titan of 0.2 | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging, Profile, Rod, Tube |
Zink | 0.2 Show Material materials with Zink of 0.2 | F | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3354 | Forging, Profile, Rod, Tube |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |