Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20.0 °C | 2.66 g/cm³ Show Material materials with Dichte of 2.66 g/cm³ | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Wire | A100 |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip | A10 | |
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
20.0 °C | 9.0 % Show Material materials with Dehnung of 9.0 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Wire | A10 | |
Elastizitätsmodul | 20.0 °C | 68.0 - 72.0 GPa Show Material materials with Elastizitätsmodul of 68.0 - 72.0 GPa | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire | |
Härte, Brinell | 20.0 °C | 75.0 [-] Show Material materials with Härte, Brinell of 75.0 [-] | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Wire | |
20.0 °C | 80.0 [-] Show Material materials with Härte, Brinell of 80.0 [-] | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Scherfestigkeit | 20.0 °C | 135.0 MPa Show Material materials with Scherfestigkeit of 135.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Wire | |
Schubmodule | 20.0 °C | 27.0 GPa Show Material materials with Schubmodule of 27.0 GPa | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire | |
Zugfestigkeit | 20.0 °C | 260.0 MPa Show Material materials with Zugfestigkeit of 260.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Wire | |
20.0 °C | 265.0 - 305.0 MPa Show Material materials with Zugfestigkeit of 265.0 - 305.0 MPa | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 2.39e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.39e-05 1/K | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire | |
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 560.0 - 655.0 °C Show Material materials with Schmelzpunkt of 560.0 - 655.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Spezifische Wärmekapazität | 20.0 °C | 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 963.0 J/(kg·K) | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire | |
Wärmeleitfähigkeit | 20.0 °C | 140.0 - 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 140.0 - 160.0 W/(m·K) | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 20000000.0 - 23000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 20000000.0 - 23000000.0 S/m | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire | |
spezifischer Widerstand | 3.3e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.3e-08 - 5e-08 Ω·m | Typical for Wrought 5000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.3 Show Material materials with Chrom of 0.3 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire |
Eisen | 0.4 Show Material materials with Eisen of 0.4 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire |
Kupfer | 0.1 Show Material materials with Kupfer of 0.1 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire |
Magnesium | 2.6 - 3.6 % Show Material materials with Magnesium of 2.6 - 3.6 % | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire |
Mangan | 0.5 Show Material materials with Mangan of 0.5 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire |
Silizium | 0.4 Show Material materials with Silizium of 0.4 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire |
Titan | 0.15 Show Material materials with Titan of 0.15 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire |
Zink | 0.2 Show Material materials with Zink of 0.2 | T6 | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Flat, Strip, Wire |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |