DIN 1725-1 Grade 3.3535 H28

View suppliers (7)
Want to keep this datasheet? Save it now in your required format

Description

The alloy is characterised by a good corrosion resistance. It is sea water steady and resistant to saline atmosphere. The Mg content increases the strength, but the cold forming capacity decreases. The material is nature hard, i.e. only by a cold forming and not by a purposeful heat treatment a strength increase can be attained. It is well polishable and anodisable. The splinter-giving machinability becomes better with increasing Mg content, just as the weldability. The material is used for statically loaded construction units. It is of this type of alloy the material most common used in the technology. For decorative anodising must be proceeded from the anodising quality AlMg3EQ. Application: In the apparatus engineering for pressure and compressed gas according to AD-W6/1 and VdTUEV-Werkstoffblaetter, for tanks for very low-temperatures, for heat exchangers. In the building industry for claddings, roofings, windows, doors and window walls, fittings as well as for carrying constructions according to DIN 4113. In the automobile engineering for commercial motor vehicle superstructures (sheet metal), for silo and tank trucks as well as body parts. For diaphragm disks of brake boosters, in the aircraft construction, in the building of forms predominantly for tools and devices as base, head and stamp plates as well as guide plates. For metal goods (incl. table-ware) and metal-describe, in food industry (including commercial devices), in the building of rail-mounted vehicles for equipments, in mechanical engineering for machine bodys, for housings. In shipbuilding for trunk and superstructures and equipment. For transport container (rolling barrel, large bottles to 10 l, liquid container up to 1 cubic meter in galvanized steel rack). For packing (doses, dose cover, valve disk for aerosol doses and bottle caps), for furniture (incl. camping furniture) and for joining elements (solid rivets, blind rivets, riveting nuts and screws) as well as for flexible pipes.

Related Standards

Equivalent Materials

Diese Materialdaten wurden von WIAM,AluKey zur Verfügung gestellt

Alle Daten beziehen sich auf Raumtemperatur soweit nicht anderweitig spezifiziert. SI Einheiten werden verwendt soweit nicht anderweitig spezifiziert.
Äquivalente Standards sind ähnlich zu einem oder mehreren Standards die der Anbieter angegeben hat. Manche äquivalente Standards können strikter sein oder außerhalb der Bedingungen des ursprünglichen Standards.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Eigenschaften

Allgemein

PropertyTemperatureValueConditionRelated StandardsShape

Dichte

2.66 g/cm³

Show Material materials with Dichte of 2.66 g/cm³

H28

EN 573-3, EN 485, EN 754

20.0 °C

2.66 g/cm³

Show Material materials with Dichte of 2.66 g/cm³

H28

DIN 1725-1, EN 573-3, EN 573-4

Flat

Mechanisch

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

140.0 MPa

Show Material materials with Bending Fatigue Strength of 140.0 MPa

H28

EN 573-3, EN 485, EN 754

Elastizitätsmodul

70.5 GPa

Show Material materials with Elastizitätsmodul of 70.5 GPa

H28

EN 573-3, EN 485, EN 754

20.0 °C

68.0 - 72.0 GPa

Show Material materials with Elastizitätsmodul of 68.0 - 72.0 GPa

H28

DIN 1725-1, EN 573-3, EN 573-4

Flat

Härte, Brinell

87.0 [-]

Show Material materials with Härte, Brinell of 87.0 [-]

H28

EN 573-3, EN 485

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poissonzahl

0.33 [-]

Show Material materials with Poissonzahl of 0.33 [-]

Typical for Wrought 5000 Series Aluminium

Schubmodule

26.5 GPa

Show Material materials with Schubmodule of 26.5 GPa

H28

EN 573-3, EN 485, EN 754

20.0 °C

27.0 GPa

Show Material materials with Schubmodule of 27.0 GPa

H28

DIN 1725-1, EN 573-3, EN 573-4

Flat

Zugfestigkeit

280.0 MPa

Show Material materials with Zugfestigkeit of 280.0 MPa

H28

EN 573-3, EN 754

290.0 MPa

Show Material materials with Zugfestigkeit of 290.0 MPa

H28

EN 573-3, EN 485

20.0 °C

290.0 - 330.0 MPa

Show Material materials with Zugfestigkeit of 290.0 - 330.0 MPa

H28

DIN 1725-1, EN 573-3, EN 573-4

Flat

Thermisch

PropertyTemperatureValueConditionRelated StandardsShapeComment

Koeffizient der thermischen Ausdehnung

20 °C

2.3899999999999998e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3899999999999998e-05 1/K

H28

EN 573-3, EN 485, EN 754

100 °C

2.3899999999999998e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3899999999999998e-05 1/K

H28

EN 573-3, EN 485, EN 754

100.0 °C

2.39e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.39e-05 1/K

H28

DIN 1725-1, EN 573-3, EN 573-4

Flat

Max. Betriebstemperatur

150.0 °C

Show Material materials with Max. Betriebstemperatur of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Schmelzpunkt

610.0 - 640.0 °C

Show Material materials with Schmelzpunkt of 610.0 - 640.0 °C

H28

EN 573-3, EN 485, EN 754

Spezifische Wärmekapazität

20.0 °C

963.0 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 963.0 J/(kg·K)

H28

DIN 1725-1, EN 573-3, EN 573-4

Flat

Wärmeleitfähigkeit

20.0 °C

140.0 - 160.0 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 140.0 - 160.0 W/(m·K)

H28

DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754

Flat

Elektrisch

PropertyTemperatureValueConditionRelated StandardsShape

Elektrische Leitfähigkeit

20.0 °C

20000000.0 - 23000000.0 S/m

Show Material materials with Elektrische Leitfähigkeit of 20000000.0 - 23000000.0 S/m

H28

DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754

Flat

spezifischer Widerstand

4.35e-08 - 5e-08 Ω·m

Show Material materials with spezifischer Widerstand of 4.35e-08 - 5e-08 Ω·m

H28

EN 573-3, EN 485, EN 754

Chemical properties

PropertyValueConditionRelated StandardsShape

Chrom

0.3

Show Material materials with Chrom of 0.3

H28

DIN 1725-1, EN 573-3, EN 573-4

Flat

Eisen

0.4 %

Show Material materials with Eisen of 0.4 %

H28

DIN 1725-1, EN 573-3, EN 573-4

Flat

0.40 %

Show Material materials with Eisen of 0.40 %

H28

EN 573-3, EN 485, EN 754

Kupfer

0.1 %

Show Material materials with Kupfer of 0.1 %

H28

DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754

Flat

Magnesium

2.6 - 3.6 %

Show Material materials with Magnesium of 2.6 - 3.6 %

H28

DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754

Flat

Mangan

0.5 %

Show Material materials with Mangan of 0.5 %

H28

DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754

Flat

Silizium

0.4 %

Show Material materials with Silizium of 0.4 %

H28

DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754

Flat

Titan

0.15 %

Show Material materials with Titan of 0.15 %

H28

DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754

Flat

Zink

0.2 %

Show Material materials with Zink of 0.2 %

H28

DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 754

Flat

Technological properties

Property
Anodizing

decorative: gut (EQ: sehr gut), Protective: very good

Brazing

hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor

Corrosion properties

Seawater: very good to good, weathering: very good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12)