Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20.0 °C | 2.75 g/cm³ Show Material materials with Dichte of 2.75 g/cm³ | T42 | WL 3.1124-1, DIN 1725-1 | Wire |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastizitätsmodul | 20.0 °C | 71.1 GPa Show Material materials with Elastizitätsmodul of 71.1 GPa | T42 | WL 3.1124-1, DIN 1725-1 | Wire | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Scherfestigkeit | 20.0 °C | 195.0 MPa Show Material materials with Scherfestigkeit of 195.0 MPa | T42 | WL 3.1124-1, DIN 1725-1 | Wire | |
Schubmodule | 26.0 - 27.5 GPa Show Material materials with Schubmodule of 26.0 - 27.5 GPa | Typical for Wrought 2000 Series Aluminium |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 1.6e-05 - 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6e-05 - 2.4e-05 1/K | Typical for Wrought 2000 Series Aluminium | ||||
Schmelzpunkt | 500.0 - 650.0 °C Show Material materials with Schmelzpunkt of 500.0 - 650.0 °C | Typical for Wrought 2000 Series Aluminium | ||||
Spezifische Wärmekapazität | 20.0 °C | 920.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 920.0 J/(kg·K) | T42 | WL 3.1124-1, DIN 1725-1 | Wire | |
Wärmeleitfähigkeit | 20.0 °C | 150.0 - 180.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 150.0 - 180.0 W/(m·K) | T42 | WL 3.1124-1, DIN 1725-1 | Wire |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 21000000.0 - 25000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 21000000.0 - 25000000.0 S/m | T42 | WL 3.1124-1, DIN 1725-1 | Wire | |
spezifischer Widerstand | 3.4e-08 - 6e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.4e-08 - 6e-08 Ω·m | Typical for Wrought 2000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.1 Show Material materials with Chrom of 0.1 | T42 | WL 3.1124-1, DIN 1725-1 | Wire |
Eisen | 0.7 Show Material materials with Eisen of 0.7 | T42 | WL 3.1124-1, DIN 1725-1 | Wire |
Kupfer | 2.2 - 3.0 % Show Material materials with Kupfer of 2.2 - 3.0 % | T42 | WL 3.1124-1, DIN 1725-1 | Wire |
Magnesium | 0.2 - 0.5 % Show Material materials with Magnesium of 0.2 - 0.5 % | T42 | WL 3.1124-1, DIN 1725-1 | Wire |
Mangan | 0.2 Show Material materials with Mangan of 0.2 | T42 | WL 3.1124-1, DIN 1725-1 | Wire |
Silizium | 0.8 Show Material materials with Silizium of 0.8 | T42 | WL 3.1124-1, DIN 1725-1 | Wire |
Zink | 0.25 Show Material materials with Zink of 0.25 | T42 | WL 3.1124-1, DIN 1725-1 | Wire |
Technological properties
Property | ||
---|---|---|
Workability | Moderate Workability |