Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | Typical for Wrought 6000 Series Aluminium |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | T651 | WL 3.3214-1, DIN 1725-1 | Plate | Transverse |
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | T651 | WL 3.3214-1, DIN 1725-1 | Plate | Transverse | |
20.0 °C | 9.0 % Show Material materials with Dehnung of 9.0 % | T651 | WL 3.3214-1, DIN 1725-1 | Plate | Transverse | |
20.0 °C | 9.0 % Show Material materials with Dehnung of 9.0 % | T651 | WL 3.3214-1, DIN 1725-1 | Rod | ||
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | T651 | WL 3.3214-1, DIN 1725-1 | A50 Transverse | ||
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | T651 | WL 3.3214-1, DIN 1725-1 | A50 Transverse | ||
20.0 °C | 18.0 % Show Material materials with Dehnung of 18.0 % | T651 | WL 3.3214-1, DIN 1725-1 | A50 Transverse | ||
20.0 °C | 18.0 % Show Material materials with Dehnung of 18.0 % | T651 | WL 3.3214-1, DIN 1725-1 | Transverse | ||
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | Typical for Wrought 6000 Series Aluminium | ||||
Härte, Brinell | 20.0 °C | 40.0 [-] Show Material materials with Härte, Brinell of 40.0 [-] | T651 | WL 3.3214-1, DIN 1725-1 | Transverse | |
20.0 °C | 90.0 [-] Show Material materials with Härte, Brinell of 90.0 [-] | T651 | WL 3.3214-1, DIN 1725-1 | Plate | Transverse | |
20.0 °C | 90.0 [-] Show Material materials with Härte, Brinell of 90.0 [-] | T651 | WL 3.3214-1, DIN 1725-1 | Rod | ||
Plane-Strain Fracture Toughnes | 20.0 °C | 23.4 - 32.9 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 23.4 - 32.9 MPa·√m | T651 | WL 3.3214-1, DIN 1725-1 | ||
20.0 °C | 23.4 - 29.4 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 23.4 - 29.4 MPa·√m | T651 | WL 3.3214-1, DIN 1725-1 | |||
20.0 °C | 23.4 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 23.4 MPa·√m | T651 | WL 3.3214-1, DIN 1725-1 | |||
20.0 °C | 29.4 - 32.9 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.4 - 32.9 MPa·√m | T651 | WL 3.3214-1, DIN 1725-1 | |||
20.0 °C | 29.4 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.4 MPa·√m | T651 | WL 3.3214-1, DIN 1725-1 | |||
20.0 °C | 32.9 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 32.9 MPa·√m | T651 | WL 3.3214-1, DIN 1725-1 | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Schubmodule | 26.0 - 26.5 GPa Show Material materials with Schubmodule of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | ||||
Zugfestigkeit | 20.0 °C | 150.0 MPa Show Material materials with Zugfestigkeit of 150.0 MPa | T651 | WL 3.3214-1, DIN 1725-1 | Transverse | |
20.0 °C | 290.0 MPa Show Material materials with Zugfestigkeit of 290.0 MPa | T651 | WL 3.3214-1, DIN 1725-1 | Plate | Transverse | |
20.0 °C | 290.0 MPa Show Material materials with Zugfestigkeit of 290.0 MPa | T651 | WL 3.3214-1, DIN 1725-1 | Rod |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 1.6e-05 - 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6e-05 - 2.4e-05 1/K | Typical for Wrought 6000 Series Aluminium |
Schmelzpunkt | 555.0 - 655.0 °C Show Material materials with Schmelzpunkt of 555.0 - 655.0 °C | Typical for Wrought 6000 Series Aluminium |
Spezifische Wärmekapazität | 887.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 887.0 - 963.0 J/(kg·K) | Typical for Wrought 6000 Series Aluminium |
Wärmeleitfähigkeit | 170.0 - 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 170.0 - 220.0 W/(m·K) | Typical for Wrought 6000 Series Aluminium |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 21000000.0 - 34000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 21000000.0 - 34000000.0 S/m | Typical for Wrought 6000 Series Aluminium |
spezifischer Widerstand | 2.9e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.9e-08 - 5e-08 Ω·m | Typical for Wrought 6000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.04 - 0.35 % Show Material materials with Chrom of 0.04 - 0.35 % | T651 | WL 3.3214-1, DIN 1725-1 | Plate, Rod |
Eisen | 0.7 Show Material materials with Eisen of 0.7 | T651 | WL 3.3214-1, DIN 1725-1 | Plate, Rod |
Kupfer | 0.15 - 0.4 % Show Material materials with Kupfer of 0.15 - 0.4 % | T651 | WL 3.3214-1, DIN 1725-1 | Plate, Rod |
Magnesium | 0.8 - 1.2 % Show Material materials with Magnesium of 0.8 - 1.2 % | T651 | WL 3.3214-1, DIN 1725-1 | Plate, Rod |
Mangan | 0.15 Show Material materials with Mangan of 0.15 | T651 | WL 3.3214-1, DIN 1725-1 | Plate, Rod |
Silizium | 0.4 - 0.8 % Show Material materials with Silizium of 0.4 - 0.8 % | T651 | WL 3.3214-1, DIN 1725-1 | Plate, Rod |
Titan | 0.15 Show Material materials with Titan of 0.15 | T651 | WL 3.3214-1, DIN 1725-1 | Plate, Rod |
Zink | 0.25 Show Material materials with Zink of 0.25 | T651 | WL 3.3214-1, DIN 1725-1 | Plate, Rod |
Technological properties
Property | ||
---|---|---|
Workability | Excellent workability. |