Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.73 g/cm³ Show Material materials with Dichte of 2.73 g/cm³ | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 2.73 g/cm³ Show Material materials with Dichte of 2.73 g/cm³ | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 65.0 MPa Show Material materials with Bending Fatigue Strength of 65.0 MPa | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
Biegewinkel 180° | 2.0 °/t Show Material materials with Biegewinkel 180° of 2.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
Biegewinkel 90° | 0.5 °/t Show Material materials with Biegewinkel 90° of 0.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
2.0 °/t Show Material materials with Biegewinkel 90° of 2.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
2.5 °/t Show Material materials with Biegewinkel 90° of 2.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
Dehnung | 1.0 % Show Material materials with Dehnung of 1.0 % | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | |
2.0 % Show Material materials with Dehnung of 2.0 % | H14 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
3.0 % Show Material materials with Dehnung of 3.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
4.0 % Show Material materials with Dehnung of 4.0 % | H14 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A100 | ||
6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A100 | ||
20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | H14 | EN 573-3 | Foil | A50 | |
20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | H14 | EN 573-3 | Foil | A100 | |
20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | H14 | EN 573-3 | Sheet, Flat | A50 | |
20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H14 | EN 573-3 | Rod, Tube, Flat | A50 | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Sheet | ||
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Flat | Transverse | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Wire | A100 | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3 | Sheet | A50 | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3 | Rod, Tube | ||
Elastizitätsmodul | -270.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | |
69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
20.0 °C | 60.0 - 70.0 GPa Show Material materials with Elastizitätsmodul of 60.0 - 70.0 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
20.0 °C | 60.0 - 65.0 GPa Show Material materials with Elastizitätsmodul of 60.0 - 65.0 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
20.0 °C | 60.0 - 69.5 GPa Show Material materials with Elastizitätsmodul of 60.0 - 69.5 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
20.0 °C | 60.0 - 69.0 GPa Show Material materials with Elastizitätsmodul of 60.0 - 69.0 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
20.0 °C | 65.0 - 70.0 GPa Show Material materials with Elastizitätsmodul of 65.0 - 70.0 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
20.0 °C | 65.0 - 69.5 GPa Show Material materials with Elastizitätsmodul of 65.0 - 69.5 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
20.0 °C | 65.0 - 69.0 GPa Show Material materials with Elastizitätsmodul of 65.0 - 69.0 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
20.0 °C | 69.0 - 70.0 GPa Show Material materials with Elastizitätsmodul of 69.0 - 70.0 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
20.0 °C | 69.0 - 69.5 GPa Show Material materials with Elastizitätsmodul of 69.0 - 69.5 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
20.0 °C | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
20.0 °C | 69.5 - 70.0 GPa Show Material materials with Elastizitätsmodul of 69.5 - 70.0 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
20.0 °C | 69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
50.0 °C | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
100.0 °C | 68.0 GPa Show Material materials with Elastizitätsmodul of 68.0 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
150.0 °C | 66.0 GPa Show Material materials with Elastizitätsmodul of 66.0 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
200.0 °C | 63.0 GPa Show Material materials with Elastizitätsmodul of 63.0 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
250.0 °C | 57.0 GPa Show Material materials with Elastizitätsmodul of 57.0 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
300.0 °C | 50.0 GPa Show Material materials with Elastizitätsmodul of 50.0 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
Härte, Brinell | 46.0 [-] Show Material materials with Härte, Brinell of 46.0 [-] | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 40.0 [-] Show Material materials with Härte, Brinell of 40.0 [-] | H14 | EN 573-3 | Rod, Tube | ||
20.0 °C | 46.0 [-] Show Material materials with Härte, Brinell of 46.0 [-] | H14 | EN 573-3 | Flat, Sheet | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | |
Schubmodule | 26.1 GPa Show Material materials with Schubmodule of 26.1 GPa | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 24.0 - 26.5 GPa Show Material materials with Schubmodule of 24.0 - 26.5 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
20.0 °C | 24.0 - 26.1 GPa Show Material materials with Schubmodule of 24.0 - 26.1 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
20.0 °C | 26.1 - 26.5 GPa Show Material materials with Schubmodule of 26.1 - 26.5 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
20.0 °C | 26.1 GPa Show Material materials with Schubmodule of 26.1 GPa | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | ||
Zugfestigkeit | 20.0 °C | 120.0 - 185.0 MPa Show Material materials with Zugfestigkeit of 120.0 - 185.0 MPa | H14 | EN 573-3 | Sheet | |
20.0 °C | 120.0 - 160.0 MPa Show Material materials with Zugfestigkeit of 120.0 - 160.0 MPa | H14 | EN 573-3 | Sheet | ||
20.0 °C | 130.0 - 165.0 MPa Show Material materials with Zugfestigkeit of 130.0 - 165.0 MPa | H14 | EN 573-3, EN 754 | Rod, Tube, Strip, Sheet, Plate, Foil, Wire, Bar | ||
20.0 °C | 135.0 - 180.0 MPa Show Material materials with Zugfestigkeit of 135.0 - 180.0 MPa | H14 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Foil, Tube, Bar | ||
20.0 °C | 140.0 - 180.0 MPa Show Material materials with Zugfestigkeit of 140.0 - 180.0 MPa | H14 | EN 573-3 | Foil | ||
20.0 °C | 145.0 - 185.0 MPa Show Material materials with Zugfestigkeit of 145.0 - 185.0 MPa | H14 | EN 573-3, EN 485, EN 541, EN 683 | Foil, Sheet, Flat, Strip, Plate, Wire, Tube, Bar | ||
20.0 °C | 145.0 - 160.0 MPa Show Material materials with Zugfestigkeit of 145.0 - 160.0 MPa | H14 | EN 573-3 | Sheet | ||
20.0 °C | 145.0 - 185.0 MPa Show Material materials with Zugfestigkeit of 145.0 - 185.0 MPa | H14 | EN 573-3 | Flat | Transverse |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.1499999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1499999999999997e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar |
-50.0 °C | 2.15e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.15e-05 1/K | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | |
20 °C | 2.1499999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1499999999999997e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3199999999999998e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20 °C | 2.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.41e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | |
20 °C | 2.52e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.52e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3199999999999998e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
100.0 °C | 2.32e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.32e-05 1/K | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | |
200 °C | 2.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.41e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | |
200.0 °C | 2.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.41e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | |
300 °C | 2.52e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.52e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | |
300.0 °C | 2.52e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.52e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | |
Schmelzpunkt | 640.0 - 655.0 °C Show Material materials with Schmelzpunkt of 640.0 - 655.0 °C | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
643.0 - 654.0 °C Show Material materials with Schmelzpunkt of 643.0 - 654.0 °C | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
Spezifische Wärmekapazität | 893.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 893.0 J/(kg·K) | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 892.0 - 893.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 892.0 - 893.0 J/(kg·K) | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | |
20.0 °C | 892.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 892.0 J/(kg·K) | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | |
20.0 °C | 893.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 893.0 J/(kg·K) | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | |
Wärmeleitfähigkeit | 159.0 - 193.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 159.0 - 193.0 W/(m·K) | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 160.0 - 200.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 - 200.0 W/(m·K) | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | |
20.0 °C | 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 W/(m·K) | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 24000000.0 - 29000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 24000000.0 - 29000000.0 S/m | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 22000000.0 - 29000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 22000000.0 - 29000000.0 S/m | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | |
20.0 °C | 23000000.0 - 29000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 29000000.0 S/m | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | |
spezifischer Widerstand | 3.45e-08 - 4.17e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.45e-08 - 4.17e-08 Ω·m | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
3.45e-08 - 4.35e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.45e-08 - 4.35e-08 Ω·m | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 3.4e-08 - 4.1e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.4e-08 - 4.1e-08 Ω·m | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | |
20.0 °C | 3.4e-08 - 4.5e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.4e-08 - 4.5e-08 Ω·m | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | |
20.0 °C | 4.1e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.1e-08 Ω·m | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire | |
20.0 °C | 4.1e-08 - 4.5e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.1e-08 - 4.5e-08 Ω·m | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Eisen | 0.7 % Show Material materials with Eisen of 0.7 % | H14 | EN 573-3 | Rod, Sheet, Flat, Foil, Tube, Wire |
0.70 % Show Material materials with Eisen of 0.70 % | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
Kupfer | 0.05 - 0.2 % Show Material materials with Kupfer of 0.05 - 0.2 % | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Rod, Sheet, Flat, Foil, Tube, Wire, Strip, Plate, Bar |
Mangan | 1.0 - 1.5 % Show Material materials with Mangan of 1.0 - 1.5 % | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Rod, Sheet, Flat, Foil, Tube, Wire, Strip, Plate, Bar |
Silizium | 0.6 % Show Material materials with Silizium of 0.6 % | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Rod, Sheet, Flat, Foil, Tube, Wire, Strip, Plate, Bar |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | H14 | EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754 | Rod, Sheet, Flat, Foil, Tube, Wire, Strip, Plate, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (O) / very good (H12) |