EN 573-3 Grade AW-3003 O

View suppliers (43)
Want to keep this datasheet? Save it now in your required format

Description

Aluminum EN AW-3003 is a popular alloy that offers customers very good atmospheric corrosion resistance and moderate strength. Aluminum 3003 offers good machinability for aluminum alloys, though it is not heat treatable. Unlike other aluminum alloys, EN AW-3003 is weldable by conventional welding methods. It also takes cold and hot working well and has generally better mechanical properties when compared to 1000 series aluminum alloys.

Related Standards

Equivalent Materials

Diese Materialdaten wurden von WIAM,AluKey,Aludium zur Verfügung gestellt

Alle Daten beziehen sich auf Raumtemperatur soweit nicht anderweitig spezifiziert. SI Einheiten werden verwendt soweit nicht anderweitig spezifiziert.
Äquivalente Standards sind ähnlich zu einem oder mehreren Standards die der Anbieter angegeben hat. Manche äquivalente Standards können strikter sein oder außerhalb der Bedingungen des ursprünglichen Standards.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Eigenschaften

Allgemein

PropertyTemperatureValueConditionRelated StandardsShape

Dichte

2.73 g/cm³

Show Material materials with Dichte of 2.73 g/cm³

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

2.73 g/cm³

Show Material materials with Dichte of 2.73 g/cm³

O

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2

Profile, Foil, Rod, Sheet, Flat, Tube, Wire, Coil, Sheet, Foil

Abmessung

PropertyValueConditionRelated StandardsThicknessShape

Dicke

0.2 mm

Show Material materials with Dicke of 0.2 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2

0.2 mm

Coil, Sheet, Foil

2.0 mm

Show Material materials with Dicke of 2.0 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2

2.0 mm

Coil, Sheet, Foil

Mechanisch

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

50.0 MPa

Show Material materials with Bending Fatigue Strength of 50.0 MPa

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

Biegewinkel 180°

0 °/t

Show Material materials with Biegewinkel 180° of 0 °/t

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2

Coil, Sheet, Foil

1.0 °/t

Show Material materials with Biegewinkel 180° of 1.0 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

Biegewinkel 90°

1.0 °/t

Show Material materials with Biegewinkel 90° of 1.0 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

1.5 °/t

Show Material materials with Biegewinkel 90° of 1.5 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

Dehnung

-196.0 °C

46.0 %

Show Material materials with Dehnung of 46.0 %

O

EN 573-3

-80.0 °C

42.0 %

Show Material materials with Dehnung of 42.0 %

O

EN 573-3

-28.0 °C

41.0 %

Show Material materials with Dehnung of 41.0 %

O

EN 573-3

1 %

Show Material materials with Dehnung of 1 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2

Coil, Sheet, Foil

A50

7.0 %

Show Material materials with Dehnung of 7.0 %

O

EN 573-3, EN 546

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

8.0 %

Show Material materials with Dehnung of 8.0 %

O

EN 573-3, EN 546

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

10.0 %

Show Material materials with Dehnung of 10.0 %

O

EN 573-3, EN 683

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

12.0 %

Show Material materials with Dehnung of 12.0 %

O

EN 573-3, EN 546

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

13.0 %

Show Material materials with Dehnung of 13.0 %

O

EN 573-3, EN 683

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

15.0 %

Show Material materials with Dehnung of 15.0 %

O

EN 573-3, EN 485, EN 546, EN 683

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

16.0 %

Show Material materials with Dehnung of 16.0 %

O

EN 573-3, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

17.0 %

Show Material materials with Dehnung of 17.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

18.0 %

Show Material materials with Dehnung of 18.0 %

O

EN 573-3

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 %

Show Material materials with Dehnung of 20.0 %

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

21.0 %

Show Material materials with Dehnung of 21.0 %

O

EN 573-3

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

23.0 %

Show Material materials with Dehnung of 23.0 %

O

EN 573-3

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

23.0 %

Show Material materials with Dehnung of 23.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A100

23.0 %

Show Material materials with Dehnung of 23.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

24.0 %

Show Material materials with Dehnung of 24.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

25.0 %

Show Material materials with Dehnung of 25.0 %

O

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A100

35.0 %

Show Material materials with Dehnung of 35.0 %

O

EN 573-3, EN 1301

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

5.0 %

Show Material materials with Dehnung of 5.0 %

O

EN 573-3

Foil

A100

20.0 °C

5.0 %

Show Material materials with Dehnung of 5.0 %

O

EN 573-3

Foil

A50

20.0 °C

6.0 %

Show Material materials with Dehnung of 6.0 %

O

EN 573-3

Foil

A100

20.0 °C

6.0 %

Show Material materials with Dehnung of 6.0 %

O

EN 573-3

Foil

A50

20.0 °C

7.0 %

Show Material materials with Dehnung of 7.0 %

O

EN 573-3

Foil

A100

20.0 °C

7.0 %

Show Material materials with Dehnung of 7.0 %

O

EN 573-3

Foil

A50

20.0 °C

8.0 %

Show Material materials with Dehnung of 8.0 %

O

EN 573-3

Foil

A100

20.0 °C

8.0 %

Show Material materials with Dehnung of 8.0 %

O

EN 573-3

Foil

A50

20.0 °C

10.0 %

Show Material materials with Dehnung of 10.0 %

O

EN 573-3

Foil

A100

20.0 °C

10.0 %

Show Material materials with Dehnung of 10.0 %

O

EN 573-3

Foil

A50

20.0 °C

12.0 %

Show Material materials with Dehnung of 12.0 %

O

EN 573-3

Foil

A100

20.0 °C

12.0 %

Show Material materials with Dehnung of 12.0 %

O

EN 573-3

Foil

A50

20.0 °C

13.0 %

Show Material materials with Dehnung of 13.0 %

O

EN 573-3

Foil

A100

20.0 °C

13.0 %

Show Material materials with Dehnung of 13.0 %

O

EN 573-3

Foil

A50

20.0 °C

15.0 %

Show Material materials with Dehnung of 15.0 %

O

EN 573-3

Foil

A100

20.0 °C

15.0 %

Show Material materials with Dehnung of 15.0 %

O

EN 573-3

Foil, Flat

A50

20.0 °C

15.0 %

Show Material materials with Dehnung of 15.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

16.0 %

Show Material materials with Dehnung of 16.0 %

O

EN 573-3

Rod

A50

20.0 °C

17.0 %

Show Material materials with Dehnung of 17.0 %

O

EN 573-3

Flat

A50

20.0 °C

17.0 %

Show Material materials with Dehnung of 17.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

18.0 %

Show Material materials with Dehnung of 18.0 %

O

EN 573-3

Sheet

A50

20.0 °C

20.0 %

Show Material materials with Dehnung of 20.0 %

O

EN 573-3

Rod, Tube, Flat

A50

20.0 °C

20.0 %

Show Material materials with Dehnung of 20.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

21.0 %

Show Material materials with Dehnung of 21.0 %

O

EN 573-3

Profile, Rod

20.0 °C

23.0 %

Show Material materials with Dehnung of 23.0 %

O

EN 573-3

Sheet

20.0 °C

23.0 %

Show Material materials with Dehnung of 23.0 %

O

EN 573-3

Sheet, Flat

A50

20.0 °C

23.0 %

Show Material materials with Dehnung of 23.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

23.0 %

Show Material materials with Dehnung of 23.0 %

O

EN 573-3

Flat

Transverse

20.0 °C

24.0 %

Show Material materials with Dehnung of 24.0 %

O

EN 573-3

Flat

A50

20.0 °C

24.0 %

Show Material materials with Dehnung of 24.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

25.0 %

Show Material materials with Dehnung of 25.0 %

O

EN 573-3

Rod, Tube

20.0 °C

35.0 %

Show Material materials with Dehnung of 35.0 %

O

EN 573-3

Wire

A100

20.0 °C

40.0 %

Show Material materials with Dehnung of 40.0 %

O

EN 573-3

100.0 °C

43.0 %

Show Material materials with Dehnung of 43.0 %

O

EN 573-3

150.0 °C

47.0 %

Show Material materials with Dehnung of 47.0 %

O

EN 573-3

200.0 °C

60.0 %

Show Material materials with Dehnung of 60.0 %

O

EN 573-3

260.0 °C

65.0 %

Show Material materials with Dehnung of 65.0 %

O

EN 573-3

315.0 °C

70.0 %

Show Material materials with Dehnung of 70.0 %

O

EN 573-3

370.0 °C

70.0 %

Show Material materials with Dehnung of 70.0 %

O

EN 573-3

Elastizitätsmodul

-270 °C

70.0 GPa

Show Material materials with Elastizitätsmodul of 70.0 GPa

O

EN 573-3

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat

-270.0 °C

70.0 GPa

Show Material materials with Elastizitätsmodul of 70.0 GPa

O

EN 573-3

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat

69.0 GPa

Show Material materials with Elastizitätsmodul of 69.0 GPa

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

69.5 GPa

Show Material materials with Elastizitätsmodul of 69.5 GPa

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

60.0 - 70.0 GPa

Show Material materials with Elastizitätsmodul of 60.0 - 70.0 GPa

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

60.0 - 65.0 GPa

Show Material materials with Elastizitätsmodul of 60.0 - 65.0 GPa

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

60.0 - 69.5 GPa

Show Material materials with Elastizitätsmodul of 60.0 - 69.5 GPa

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

60.0 - 69.0 GPa

Show Material materials with Elastizitätsmodul of 60.0 - 69.0 GPa

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

65.0 - 70.0 GPa

Show Material materials with Elastizitätsmodul of 65.0 - 70.0 GPa

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

65.0 - 69.5 GPa

Show Material materials with Elastizitätsmodul of 65.0 - 69.5 GPa

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

65.0 - 69.0 GPa

Show Material materials with Elastizitätsmodul of 65.0 - 69.0 GPa

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

69.0 GPa

Show Material materials with Elastizitätsmodul of 69.0 GPa

O

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat, Coil, Sheet, Foil

20.0 °C

69.0 - 70.0 GPa

Show Material materials with Elastizitätsmodul of 69.0 - 70.0 GPa

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

69.0 - 69.5 GPa

Show Material materials with Elastizitätsmodul of 69.0 - 69.5 GPa

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

69.5 GPa

Show Material materials with Elastizitätsmodul of 69.5 GPa

O

EN 573-3

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat

20.0 °C

69.5 - 70.0 GPa

Show Material materials with Elastizitätsmodul of 69.5 - 70.0 GPa

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

20 °C

70.0 GPa

Show Material materials with Elastizitätsmodul of 70.0 GPa

O

EN 573-3

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat

20.0 °C

70.0 GPa

Show Material materials with Elastizitätsmodul of 70.0 GPa

O

EN 573-3

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat

50.0 °C

69.0 GPa

Show Material materials with Elastizitätsmodul of 69.0 GPa

O

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat, Coil, Sheet, Foil

100.0 °C

68.0 GPa

Show Material materials with Elastizitätsmodul of 68.0 GPa

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

150.0 °C

66.0 GPa

Show Material materials with Elastizitätsmodul of 66.0 GPa

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

200.0 °C

63.0 GPa

Show Material materials with Elastizitätsmodul of 63.0 GPa

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

250.0 °C

57.0 GPa

Show Material materials with Elastizitätsmodul of 57.0 GPa

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

300 °C

50.0 GPa

Show Material materials with Elastizitätsmodul of 50.0 GPa

O

EN 573-3

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat

300.0 °C

50.0 GPa

Show Material materials with Elastizitätsmodul of 50.0 GPa

O

EN 573-3

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat

Härte, Brinell

28.0 [-]

Show Material materials with Härte, Brinell of 28.0 [-]

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

28.0 [-]

Show Material materials with Härte, Brinell of 28.0 [-]

O

EN 573-3

Flat, Sheet

20.0 °C

29.0 [-]

Show Material materials with Härte, Brinell of 29.0 [-]

O

EN 573-3

Rod, Tube

20.0 °C

30.0 [-]

Show Material materials with Härte, Brinell of 30.0 [-]

O

EN 573-3

Rod, Tube

Härte, HBW

25.0 - 60.0 [-]

Show Material materials with Härte, HBW of 25.0 - 60.0 [-]

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2

Coil, Sheet, Foil

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 3000 Series Aluminium

Poissonzahl

20.0 °C

0.33 [-]

Show Material materials with Poissonzahl of 0.33 [-]

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

Schubmodule

26.0 GPa

Show Material materials with Schubmodule of 26.0 GPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2

Coil, Sheet, Foil

26.1 GPa

Show Material materials with Schubmodule of 26.1 GPa

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

24.0 - 26.5 GPa

Show Material materials with Schubmodule of 24.0 - 26.5 GPa

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

24.0 - 26.1 GPa

Show Material materials with Schubmodule of 24.0 - 26.1 GPa

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

26.1 - 26.5 GPa

Show Material materials with Schubmodule of 26.1 - 26.5 GPa

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

26.1 GPa

Show Material materials with Schubmodule of 26.1 GPa

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

Streckgrenze

-270 °C

35.0 MPa

Show Material materials with Streckgrenze of 35.0 MPa

O

EN 573-3

Profile, Rod, Tube, Sheet, Strip, Plate, Foil, Wire, Bar, Flat

RP02

-270.0 °C

35.0 MPa

Show Material materials with Streckgrenze of 35.0 MPa

O

EN 573-3

Profile, Rod, Tube, Sheet, Strip, Plate, Foil, Wire, Bar, Flat

RP02

-196.0 °C

60.0 MPa

Show Material materials with Streckgrenze of 60.0 MPa

O

EN 573-3

Wire

RP02

-80.0 °C

50.0 MPa

Show Material materials with Streckgrenze of 50.0 MPa

O

EN 573-3

RP02

-28.0 °C

45.0 MPa

Show Material materials with Streckgrenze of 45.0 MPa

O

EN 573-3

RP02

35.0 MPa

Show Material materials with Streckgrenze of 35.0 MPa

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

RP02

35 MPa

Show Material materials with Streckgrenze of 35 MPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2

Coil, Sheet, Foil

60.0 MPa

Show Material materials with Streckgrenze of 60.0 MPa

O

EN 573-3, EN 1301

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

RP02

80.0 MPa

Show Material materials with Streckgrenze of 80.0 MPa

O

EN 573-3, EN 683

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

RP02

20.0 °C

35.0 MPa

Show Material materials with Streckgrenze of 35.0 MPa

O

EN 573-3

Profile, Rod, Tube, Sheet, Strip, Plate, Foil, Wire, Bar, Flat

RP02

20 °C

35.0 MPa

Show Material materials with Streckgrenze of 35.0 MPa

O

EN 573-3

Profile, Rod, Tube, Sheet, Strip, Plate, Foil, Wire, Bar, Flat

RP02

20.0 °C

35.0 - 40.0 MPa

Show Material materials with Streckgrenze of 35.0 - 40.0 MPa

O

EN 573-3

RP02

20.0 °C

35.0 MPa

Show Material materials with Streckgrenze of 35.0 MPa

O

EN 573-3

Flat

RP02 Transverse

20.0 °C

40.0 MPa

Show Material materials with Streckgrenze of 40.0 MPa

O

EN 573-3

RP02

20.0 °C

60.0 MPa

Show Material materials with Streckgrenze of 60.0 MPa

O

EN 573-3

Wire

RP02

20.0 °C

65.0 MPa

Show Material materials with Streckgrenze of 65.0 MPa

O

EN 573-3

Foil

RP02

20.0 °C

80.0 MPa

Show Material materials with Streckgrenze of 80.0 MPa

O

EN 573-3

Foil

RP02

50 °C

35.0 MPa

Show Material materials with Streckgrenze of 35.0 MPa

O

EN 573-3

Profile, Rod, Tube, Sheet, Strip, Plate, Foil, Wire, Bar, Flat

RP02

50.0 °C

35.0 MPa

Show Material materials with Streckgrenze of 35.0 MPa

O

EN 573-3

Profile, Rod, Tube, Sheet, Strip, Plate, Foil, Wire, Bar, Flat

RP02

100.0 °C

40.0 MPa

Show Material materials with Streckgrenze of 40.0 MPa

O

EN 573-3

RP02

150.0 °C

35.0 MPa

Show Material materials with Streckgrenze of 35.0 MPa

O

EN 573-3

Profile, Rod, Tube, Sheet, Strip, Plate, Foil, Wire, Bar, Flat

RP02

200.0 °C

30.0 MPa

Show Material materials with Streckgrenze of 30.0 MPa

O

EN 573-3

RP02

260.0 °C

25.0 MPa

Show Material materials with Streckgrenze of 25.0 MPa

O

EN 573-3

RP02

315.0 °C

15.0 MPa

Show Material materials with Streckgrenze of 15.0 MPa

O

EN 573-3

RP02

370.0 °C

10.0 MPa

Show Material materials with Streckgrenze of 10.0 MPa

O

EN 573-3

RP02

Zugfestigkeit

-196.0 °C

230.0 MPa

Show Material materials with Zugfestigkeit of 230.0 MPa

O

EN 573-3

-80.0 °C

140.0 MPa

Show Material materials with Zugfestigkeit of 140.0 MPa

O

EN 573-3

-28.0 °C

120.0 MPa

Show Material materials with Zugfestigkeit of 120.0 MPa

O

EN 573-3

95.0 MPa

Show Material materials with Zugfestigkeit of 95.0 MPa

O

EN 573-3

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

95 MPa

Show Material materials with Zugfestigkeit of 95 MPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2

Coil, Sheet, Foil

100.0 MPa

Show Material materials with Zugfestigkeit of 100.0 MPa

O

EN 573-3

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

130.0 MPa

Show Material materials with Zugfestigkeit of 130.0 MPa

O

EN 573-3, EN 1301

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

80.0 - 130.0 MPa

Show Material materials with Zugfestigkeit of 80.0 - 130.0 MPa

O

EN 573-3

Foil

20.0 °C

85.0 - 135.0 MPa

Show Material materials with Zugfestigkeit of 85.0 - 135.0 MPa

O

EN 573-3, EN 546, EN 683

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

95.0 MPa

Show Material materials with Zugfestigkeit of 95.0 MPa

O

EN 573-3

Profile, Rod

20.0 °C

95.0 - 130.0 MPa

Show Material materials with Zugfestigkeit of 95.0 - 130.0 MPa

O

EN 573-3, EN 754

Rod, Tube, Strip, Sheet, Plate, Foil, Wire, Bar

20.0 °C

95.0 - 135.0 MPa

Show Material materials with Zugfestigkeit of 95.0 - 135.0 MPa

O

EN 573-3, EN 485, EN 755

Rod, Tube, Strip, Sheet, Plate, Foil, Wire, Bar, Flat

20.0 °C

95.0 - 135.0 MPa

Show Material materials with Zugfestigkeit of 95.0 - 135.0 MPa

O

EN 573-3

Flat

Transverse

20.0 °C

100.0 MPa

Show Material materials with Zugfestigkeit of 100.0 MPa

O

EN 573-3

Sheet

20.0 °C

110.0 MPa

Show Material materials with Zugfestigkeit of 110.0 MPa

O

EN 573-3

20.0 °C

130.0 MPa

Show Material materials with Zugfestigkeit of 130.0 MPa

O

EN 573-3

Wire

100.0 °C

90.0 MPa

Show Material materials with Zugfestigkeit of 90.0 MPa

O

EN 573-3

150.0 °C

75.0 MPa

Show Material materials with Zugfestigkeit of 75.0 MPa

O

EN 573-3

200.0 °C

60.0 MPa

Show Material materials with Zugfestigkeit of 60.0 MPa

O

EN 573-3

260.0 °C

40.0 MPa

Show Material materials with Zugfestigkeit of 40.0 MPa

O

EN 573-3

315.0 °C

30.0 MPa

Show Material materials with Zugfestigkeit of 30.0 MPa

O

EN 573-3

370.0 °C

20.0 MPa

Show Material materials with Zugfestigkeit of 20.0 MPa

O

EN 573-3

Thermisch

PropertyTemperatureValueConditionRelated StandardsShapeComment

Koeffizient der thermischen Ausdehnung

-50 °C

2.1499999999999997e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1499999999999997e-05 1/K

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

-50.0 °C

2.15e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.15e-05 1/K

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

20 °C

2.1499999999999997e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1499999999999997e-05 1/K

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20 °C

2.3199999999999998e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3199999999999998e-05 1/K

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20 °C

2.41e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.41e-05 1/K

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat

20 °C

2.52e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.52e-05 1/K

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat

100 °C

0.000023 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 0.000023 1/K

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2

Coil, Sheet, Foil

20-100°C

100 °C

2.3199999999999998e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3199999999999998e-05 1/K

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

100.0 °C

2.32e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.32e-05 1/K

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

200 °C

2.41e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.41e-05 1/K

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat

200.0 °C

2.41e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.41e-05 1/K

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat

300 °C

2.52e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.52e-05 1/K

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat

300.0 °C

2.52e-05 1/K

Show Material materials with Koeffizient der thermischen Ausdehnung of 2.52e-05 1/K

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat

Schmelzpunkt

640.0 - 655.0 °C

Show Material materials with Schmelzpunkt of 640.0 - 655.0 °C

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

643.0 - 654.0 °C

Show Material materials with Schmelzpunkt of 643.0 - 654.0 °C

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

Spezifische Wärmekapazität

893.0 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 893.0 J/(kg·K)

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

892.0 - 893.0 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 892.0 - 893.0 J/(kg·K)

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

892.0 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 892.0 J/(kg·K)

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

893.0 J/(kg·K)

Show Material materials with Spezifische Wärmekapazität of 893.0 J/(kg·K)

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

Wärmeleitfähigkeit

159.0 - 193.0 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 159.0 - 193.0 W/(m·K)

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

176 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 176 W/(m·K)

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2

Coil, Sheet, Foil

20.0 °C

160.0 - 200.0 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 160.0 - 200.0 W/(m·K)

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat

20.0 °C

160.0 W/(m·K)

Show Material materials with Wärmeleitfähigkeit of 160.0 W/(m·K)

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

Elektrisch

PropertyTemperatureValueConditionRelated StandardsShape

Elektrische Leitfähigkeit

24000000.0 - 29000000.0 S/m

Show Material materials with Elektrische Leitfähigkeit of 24000000.0 - 29000000.0 S/m

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

22000000.0 - 29000000.0 S/m

Show Material materials with Elektrische Leitfähigkeit of 22000000.0 - 29000000.0 S/m

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

23000000.0 - 29000000.0 S/m

Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 29000000.0 S/m

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Profile, Rod, Flat

spezifischer Widerstand

3.4e-08 Ω·m

Show Material materials with spezifischer Widerstand of 3.4e-08 Ω·m

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2

Coil, Sheet, Foil

3.45e-08 - 4.17e-08 Ω·m

Show Material materials with spezifischer Widerstand of 3.45e-08 - 4.17e-08 Ω·m

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

3.45e-08 - 4.35e-08 Ω·m

Show Material materials with spezifischer Widerstand of 3.45e-08 - 4.35e-08 Ω·m

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

3.4e-08 - 4.1e-08 Ω·m

Show Material materials with spezifischer Widerstand of 3.4e-08 - 4.1e-08 Ω·m

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

3.4e-08 - 4.5e-08 Ω·m

Show Material materials with spezifischer Widerstand of 3.4e-08 - 4.5e-08 Ω·m

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

4.1e-08 Ω·m

Show Material materials with spezifischer Widerstand of 4.1e-08 Ω·m

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

4.1e-08 - 4.5e-08 Ω·m

Show Material materials with spezifischer Widerstand of 4.1e-08 - 4.5e-08 Ω·m

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

Chemical properties

PropertyValueConditionRelated StandardsShape

Eisen

0.7 %

Show Material materials with Eisen of 0.7 %

O

EN 573-3

Profile, Foil, Rod, Sheet, Flat, Tube, Wire

0.70 %

Show Material materials with Eisen of 0.70 %

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

0.7 %

Show Material materials with Eisen of 0.7 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2

Coil, Sheet, Foil

Kupfer

0.05 - 0.2 %

Show Material materials with Kupfer of 0.05 - 0.2 %

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2

Profile, Foil, Rod, Sheet, Flat, Tube, Wire, Strip, Plate, Bar, Coil, Sheet, Foil

Mangan

1.0 - 1.5 %

Show Material materials with Mangan of 1.0 - 1.5 %

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2

Profile, Foil, Rod, Sheet, Flat, Tube, Wire, Strip, Plate, Bar, Coil, Sheet, Foil

Silizium

0.6 %

Show Material materials with Silizium of 0.6 %

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Profile, Foil, Rod, Sheet, Flat, Tube, Wire, Strip, Plate, Bar

0.6 %

Show Material materials with Silizium of 0.6 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2

Coil, Sheet, Foil

Zink

0.1 %

Show Material materials with Zink of 0.1 %

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Profile, Foil, Rod, Sheet, Flat, Tube, Wire, Strip, Plate, Bar

0.1 %

Show Material materials with Zink of 0.1 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2

Coil, Sheet, Foil

Technological properties

Property
Anodizing

decorative: sufficient, Protective: very good

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing Quality; Electronic devices: Housing of devices; Heat exchangers: Fins, Heat exchangers, General appliacations; Tubes: Industrial tubes, Flexible tube, Pipes; Wind energy: Nacelle coverings, Rotor, Hub, Stairs; Cosmetics: Cosmetics pieces; Semi-rigid and corrugated: Smooth wall; Automotive trim: Interior trims; Components: Heat shields, Automotive fins, Heat exchangers, General transportation

Brazing

hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good

Corrosion properties

Seawater: good, weathering: very good

Welding

Very Good

Workability