Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
20.0 °C | 2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | O | EN 573-3 | Profile, Rod, Flat, Tube | |
20.0 °C | 2.69 - 2.7 g/cm³ Show Material materials with Dichte of 2.69 - 2.7 g/cm³ | O | EN 573-3 | Profile, Rod, Flat, Tube | |
20.0 °C | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | O | EN 573-3 | Profile, Rod, Flat, Tube |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Biegewinkel 180° | 0.5 °/t Show Material materials with Biegewinkel 180° of 0.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | ||
1.0 °/t Show Material materials with Biegewinkel 180° of 1.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | |||
Biegewinkel 90° | 1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | ||
1.5 °/t Show Material materials with Biegewinkel 90° of 1.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | |||
Dehnung | 15.0 % Show Material materials with Dehnung of 15.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | A50 | |
16.0 % Show Material materials with Dehnung of 16.0 % | O | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Bar | A50 | ||
18.0 % Show Material materials with Dehnung of 18.0 % | O | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | A50 | ||
18.0 % Show Material materials with Dehnung of 18.0 % | O | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Bar | A100 | ||
19.0 % Show Material materials with Dehnung of 19.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | A50 | ||
20.0 % Show Material materials with Dehnung of 20.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | A50 | ||
20.0 % Show Material materials with Dehnung of 20.0 % | O | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Tube, Bar | A100 | ||
22.0 % Show Material materials with Dehnung of 22.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | A50 | ||
24.0 % Show Material materials with Dehnung of 24.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | A50 | ||
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | O | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 18.0 % Show Material materials with Dehnung of 18.0 % | O | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 18.0 % Show Material materials with Dehnung of 18.0 % | O | EN 573-3 | Rod, Tube | ||
20.0 °C | 19.0 % Show Material materials with Dehnung of 19.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 19.0 % Show Material materials with Dehnung of 19.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 20.0 % Show Material materials with Dehnung of 20.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 20.0 % Show Material materials with Dehnung of 20.0 % | O | EN 573-3 | Profile, Tube, Rod, Flat | ||
20.0 °C | 20.0 % Show Material materials with Dehnung of 20.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 20.0 % Show Material materials with Dehnung of 20.0 % | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 22.0 % Show Material materials with Dehnung of 22.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 22.0 % Show Material materials with Dehnung of 22.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 24.0 % Show Material materials with Dehnung of 24.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 24.0 % Show Material materials with Dehnung of 24.0 % | O | EN 573-3 | Flat | A50 Transverse | |
Elastizitätsmodul | 60.0 GPa Show Material materials with Elastizitätsmodul of 60.0 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | ||
69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |||
20.0 °C | 69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | O | EN 573-3 | Profile, Rod, Flat, Tube | ||
Härte, Brinell | 29.0 [-] Show Material materials with Härte, Brinell of 29.0 [-] | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | ||
20.0 °C | 29.0 [-] Show Material materials with Härte, Brinell of 29.0 [-] | O | EN 573-3 | Flat | ||
20.0 °C | 30.0 [-] Show Material materials with Härte, Brinell of 30.0 [-] | O | EN 573-3 | Profile, Rod, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | O | EN 573-3 | Profile, Rod, Flat, Tube | |
Schubmodule | 23.8 GPa Show Material materials with Schubmodule of 23.8 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | ||
26.1 GPa Show Material materials with Schubmodule of 26.1 GPa | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |||
20.0 °C | 25.0 - 26.1 GPa Show Material materials with Schubmodule of 25.0 - 26.1 GPa | O | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 26.1 GPa Show Material materials with Schubmodule of 26.1 GPa | O | EN 573-3 | Profile, Rod, Flat, Tube | ||
Zugfestigkeit | 20.0 °C | 100.0 - 150.0 MPa Show Material materials with Zugfestigkeit of 100.0 - 150.0 MPa | O | EN 573-3, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate, Bar | |
20.0 °C | 100.0 - 145.0 MPa Show Material materials with Zugfestigkeit of 100.0 - 145.0 MPa | O | EN 573-3, EN 485, EN 754 | Rod, Tube, Flat, Strip, Sheet, Plate, Bar | ||
20.0 °C | 100.0 - 145.0 MPa Show Material materials with Zugfestigkeit of 100.0 - 145.0 MPa | O | EN 573-3 | Flat | Transverse |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.18e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.18e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat | |
-50.0 °C | 2.18e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.18e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat | ||
20 °C | 2.18e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.18e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat | ||
20 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat | ||
20 °C | 2.45e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.45e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat | ||
20 °C | 2.55e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.55e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat | ||
100 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat | ||
100.0 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat | ||
100 °C | 0.000024 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.000024 1/K | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | 20-100°C | |
200 °C | 2.45e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.45e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat | ||
200.0 °C | 2.45e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.45e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat | ||
300 °C | 2.55e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.55e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat | ||
300.0 °C | 2.55e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.55e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat | ||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 630.0 - 650.0 °C Show Material materials with Schmelzpunkt of 630.0 - 650.0 °C | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
Spezifische Wärmekapazität | 20.0 °C | 879.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 879.0 J/(kg·K) | O | EN 573-3 | Profile, Rod, Flat, Tube | |
20.0 °C | 879.0 - 899.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 879.0 - 899.0 J/(kg·K) | O | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 899.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 899.0 J/(kg·K) | O | EN 573-3 | Profile, Rod, Flat, Tube | ||
Wärmeleitfähigkeit | 168.0 - 190.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 168.0 - 190.0 W/(m·K) | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | ||
20.0 °C | 160.0 - 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 - 220.0 W/(m·K) | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar, Profile, Rod, Flat | ||
20.0 °C | 160.0 - 201.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 - 201.0 W/(m·K) | O | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 201.0 - 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 201.0 - 220.0 W/(m·K) | O | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 201.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 201.0 W/(m·K) | O | EN 573-3 | Profile, Rod, Flat, Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 23000000.0 - 31000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 31000000.0 S/m | O | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Bar |
spezifischer Widerstand | 3.23e-08 - 4.35e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.23e-08 - 4.35e-08 Ω·m | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
3.5e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.5e-08 Ω·m | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | ||
20.0 °C | 3.3e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.3e-08 Ω·m | O | EN 573-3 | Profile, Rod, Flat, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Andere | 0.05 - 0.15 % Show Material materials with Andere of 0.05 - 0.15 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip |
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | O | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Bar |
0.1 % Show Material materials with Chrom of 0.1 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
Eisen | 0.45 % Show Material materials with Eisen of 0.45 % | O | EN 573-3 | Profile, Rod, Flat, Tube |
0.45 % Show Material materials with Eisen of 0.45 % | O | EN 573-3, EN 485, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Tube, Bar, Coil, Sheet, Strip | |
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | O | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Bar |
0.05 % Show Material materials with Kupfer of 0.05 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
Magnesium | 0.7 - 1.1 % Show Material materials with Magnesium of 0.7 - 1.1 % | O | EN 573-3, EN 485, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Bar, Coil, Sheet, Strip |
Mangan | 0.15 % Show Material materials with Mangan of 0.15 % | O | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Bar |
0.15 % Show Material materials with Mangan of 0.15 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
Silizium | 0.3 % Show Material materials with Silizium of 0.3 % | O | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Bar |
0.3 % Show Material materials with Silizium of 0.3 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | O | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Bar |
0.2 % Show Material materials with Zink of 0.2 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip |
Technological properties
Property | ||
---|---|---|
Anodizing | Excellent (anodizing quality) | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels, Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Lighting: Anodizing Quality, Lacquering quality; Heat exchangers: Fins; Cosmetics: Cosmetics pieces; Pharmacy: Pharma and para-Pharma; Automotive Trim: Interior Trim, Windows frames; Components: Automotive fins, Heat exchangers | |
Brazing | Good | |
Corrosion properties | Excellent | |
Welding | Excellent | |
Workability | Good |