Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate |
2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Biegewinkel 180° | 0.5 °/t Show Material materials with Biegewinkel 180° of 0.5 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
Biegewinkel 90° | 1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
2.0 °/t Show Material materials with Biegewinkel 90° of 2.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
Dehnung | 16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | |
17.0 % Show Material materials with Dehnung of 17.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | ||
19.0 % Show Material materials with Dehnung of 19.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | ||
20.0 % Show Material materials with Dehnung of 20.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | ||
20.0 % Show Material materials with Dehnung of 20.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A100 | ||
21.0 % Show Material materials with Dehnung of 21.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | ||
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 17.0 % Show Material materials with Dehnung of 17.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 17.0 % Show Material materials with Dehnung of 17.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 19.0 % Show Material materials with Dehnung of 19.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 19.0 % Show Material materials with Dehnung of 19.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 20.0 % Show Material materials with Dehnung of 20.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 20.0 % Show Material materials with Dehnung of 20.0 % | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 20.0 % Show Material materials with Dehnung of 20.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 20.0 % Show Material materials with Dehnung of 20.0 % | H111 | EN 573-3 | Flat | ||
20.0 °C | 21.0 % Show Material materials with Dehnung of 21.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 21.0 % Show Material materials with Dehnung of 21.0 % | H111 | EN 573-3 | Flat | A50 | |
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
Härte, Brinell | 36.0 [-] Show Material materials with Härte, Brinell of 36.0 [-] | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
20.0 °C | 36.0 [-] Show Material materials with Härte, Brinell of 36.0 [-] | H111 | EN 573-3 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Schubmodule | 26.0 - 26.5 GPa Show Material materials with Schubmodule of 26.0 - 26.5 GPa | Typical for Wrought 5000 Series Aluminium | ||||
Zugfestigkeit | 20.0 °C | 130.0 - 170.0 MPa Show Material materials with Zugfestigkeit of 130.0 - 170.0 MPa | H111 | EN 573-3 | Flat | Transverse |
20.0 °C | 130.0 - 170.0 MPa Show Material materials with Zugfestigkeit of 130.0 - 170.0 MPa | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
100 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 620.0 - 650.0 °C Show Material materials with Schmelzpunkt of 620.0 - 650.0 °C | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
625.0 - 650.0 °C Show Material materials with Schmelzpunkt of 625.0 - 650.0 °C | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
Spezifische Wärmekapazität | 879.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium | ||||
Wärmeleitfähigkeit | 170.0 - 190.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 170.0 - 190.0 W/(m·K) | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
193 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 193 W/(m·K) | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate |
Elektrisch
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Elektrische Leitfähigkeit | 23000000.0 - 26000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 26000000.0 S/m | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate |
29000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 29000000.0 S/m | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
spezifischer Widerstand | 3.45e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.45e-08 Ω·m | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate |
3.85e-08 - 4.35e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.85e-08 - 4.35e-08 Ω·m | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | H111 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Eisen | 0.7 % Show Material materials with Eisen of 0.7 % | H111 | EN 573-3 | Flat |
0.70 % Show Material materials with Eisen of 0.70 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
Kupfer | 0.2 % Show Material materials with Kupfer of 0.2 % | H111 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Magnesium | 1.1 - 1.8 % Show Material materials with Magnesium of 1.1 - 1.8 % | H111 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | H111 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
0.3 % Show Material materials with Mangan of 0.3 % | H111 | EN 573-3 | Flat | |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | H111 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | H111 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |