Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate |
2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip |
Abmessung
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Biegewinkel 180° | 0 °/t Show Material materials with Biegewinkel 180° of 0 °/t | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | ||
Biegewinkel 90° | 0 °/t Show Material materials with Biegewinkel 90° of 0 °/t | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | ||
1.5 °/t Show Material materials with Biegewinkel 90° of 1.5 °/t | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
2.5 °/t Show Material materials with Biegewinkel 90° of 2.5 °/t | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
Elastizitätsmodul | 68.6 GPa Show Material materials with Elastizitätsmodul of 68.6 GPa | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | ||
69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
Härte, Brinell | 68.0 [-] Show Material materials with Härte, Brinell of 68.0 [-] | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
20.0 °C | 68.0 [-] Show Material materials with Härte, Brinell of 68.0 [-] | H18 | EN 573-3 | Flat | ||
Härte, HBW | 68 [-] Show Material materials with Härte, HBW of 68 [-] | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Schubmodule | 26.5 GPa Show Material materials with Schubmodule of 26.5 GPa | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | ||
Streckgrenze | 190.0 MPa Show Material materials with Streckgrenze of 190.0 MPa | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate | RP02 | |
190 MPa Show Material materials with Streckgrenze of 190 MPa | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |||
20.0 °C | 190.0 MPa Show Material materials with Streckgrenze of 190.0 MPa | H18 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 190.0 MPa Show Material materials with Streckgrenze of 190.0 MPa | H18 | EN 573-3 | Flat | RP02 | |
Zugfestigkeit | 220.0 MPa Show Material materials with Zugfestigkeit of 220.0 MPa | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
220 MPa Show Material materials with Zugfestigkeit of 220 MPa | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |||
20.0 °C | 220.0 MPa Show Material materials with Zugfestigkeit of 220.0 MPa | H18 | EN 573-3 | Flat | Transverse | |
20.0 °C | 220.0 MPa Show Material materials with Zugfestigkeit of 220.0 MPa | H18 | EN 573-3 | Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
100 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
100 °C | 0.000024 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.000024 1/K | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | 20-100°C | |
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 620.0 - 650.0 °C Show Material materials with Schmelzpunkt of 620.0 - 650.0 °C | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
625.0 - 650.0 °C Show Material materials with Schmelzpunkt of 625.0 - 650.0 °C | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
Spezifische Wärmekapazität | 879.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium | ||||
Wärmeleitfähigkeit | 170.0 - 190.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 170.0 - 190.0 W/(m·K) | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
192 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 192 W/(m·K) | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |||
193 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 193 W/(m·K) | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate |
Elektrisch
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Elektrische Leitfähigkeit | 23000000.0 - 26000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 26000000.0 S/m | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate |
29000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 29000000.0 S/m | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
spezifischer Widerstand | 3.4e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.4e-08 Ω·m | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip |
3.45e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.45e-08 Ω·m | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
3.85e-08 - 4.35e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.85e-08 - 4.35e-08 Ω·m | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | H18 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
0.1 % Show Material materials with Chrom of 0.1 % | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
Eisen | 0.7 % Show Material materials with Eisen of 0.7 % | H18 | EN 573-3 | Flat |
0.70 % Show Material materials with Eisen of 0.70 % | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
0.7 % Show Material materials with Eisen of 0.7 % | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
Kupfer | 0.2 % Show Material materials with Kupfer of 0.2 % | H18 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
0.2 % Show Material materials with Kupfer of 0.2 % | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
Magnesium | 1.1 - 1.8 % Show Material materials with Magnesium of 1.1 - 1.8 % | H18 | EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Flat, Strip, Sheet, Plate, Coil, Sheet, Strip |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | H18 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
0.1 % Show Material materials with Mangan of 0.1 % | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
0.3 % Show Material materials with Mangan of 0.3 % | H18 | EN 573-3 | Flat | |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | H18 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
0.4 % Show Material materials with Silizium of 0.4 % | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | H18 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
0.25 % Show Material materials with Zink of 0.25 % | H18 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip |
Technological properties
Property | ||
---|---|---|
Anodizing | Very Good (anodizing quality) | |
Application areas | Roofing: Single sheet, Sheets for composites/ sandwich Panels; Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Anodizing quality; Tubes: Industrial tubes, Pipes; Food can: Body, Lids | |
Brazing | Good | |
Corrosion properties | Excellent | |
General machinability | Fair | |
Welding | Excellent | |
Workability | Very Good |