Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 2.7 - 2.85 g/cm³ Show Material materials with Dichte of 2.7 - 2.85 g/cm³ | Typical for Wrought 7000 Series Aluminium |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | T7451 | WL 3.4144-1 | Plate | Transverse |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | T7451 | WL 3.4144-1 | Plate | Transverse | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | T7451 | WL 3.4144-1 | Plate | Transverse | |
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 9.0 % Show Material materials with Dehnung of 9.0 % | T7451 | WL 3.4144-1 | Plate | ||
Elastizitätsmodul | 69.0 - 72.0 GPa Show Material materials with Elastizitätsmodul of 69.0 - 72.0 GPa | Typical for Wrought 7000 Series Aluminium | ||||
Härte, Brinell | 20.0 °C | 135.0 [-] Show Material materials with Härte, Brinell of 135.0 [-] | T7451 | WL 3.4144-1 | Plate | Transverse |
20.0 °C | 135.0 [-] Show Material materials with Härte, Brinell of 135.0 [-] | T7451 | WL 3.4144-1 | Plate | ||
Plane-Strain Fracture Toughnes | 20.0 °C | 25.4 - 39.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.4 - 39.6 MPa·√m | T7451 | WL 3.4144-1 | Plate | |
20.0 °C | 25.4 - 34.3 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.4 - 34.3 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 25.4 - 32.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.4 - 32.6 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 25.4 - 36.3 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.4 - 36.3 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 25.4 - 30.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.4 - 30.1 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 25.4 - 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.4 - 29.0 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 25.4 - 26.9 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.4 - 26.9 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 25.4 - 25.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.4 - 25.5 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 25.4 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.4 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 25.4 - 27.2 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.4 - 27.2 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 25.5 - 39.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.5 - 39.6 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 25.5 - 34.3 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.5 - 34.3 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 25.5 - 32.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.5 - 32.6 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 25.5 - 36.3 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.5 - 36.3 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 25.5 - 30.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.5 - 30.1 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 25.5 - 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.5 - 29.0 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 25.5 - 26.9 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.5 - 26.9 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 25.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.5 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 25.5 - 27.2 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 25.5 - 27.2 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 26.9 - 39.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.9 - 39.6 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 26.9 - 34.3 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.9 - 34.3 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 26.9 - 32.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.9 - 32.6 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 26.9 - 36.3 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.9 - 36.3 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 26.9 - 30.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.9 - 30.1 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 26.9 - 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.9 - 29.0 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 26.9 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.9 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 26.9 - 27.2 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.9 - 27.2 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 27.2 - 39.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.2 - 39.6 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 27.2 - 34.3 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.2 - 34.3 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 27.2 - 32.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.2 - 32.6 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 27.2 - 36.3 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.2 - 36.3 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 27.2 - 30.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.2 - 30.1 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 27.2 - 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.2 - 29.0 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 27.2 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.2 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 29.0 - 39.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 39.6 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 29.0 - 34.3 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 34.3 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 29.0 - 32.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 32.6 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 29.0 - 36.3 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 36.3 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 29.0 - 30.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 30.1 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 30.1 - 39.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.1 - 39.6 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 30.1 - 34.3 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.1 - 34.3 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 30.1 - 32.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.1 - 32.6 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 30.1 - 36.3 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.1 - 36.3 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 30.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.1 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 32.6 - 39.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 32.6 - 39.6 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 32.6 - 34.3 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 32.6 - 34.3 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 32.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 32.6 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 32.6 - 36.3 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 32.6 - 36.3 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 34.3 - 39.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 34.3 - 39.6 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 34.3 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 34.3 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 34.3 - 36.3 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 34.3 - 36.3 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 36.3 - 39.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 36.3 - 39.6 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 36.3 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 36.3 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 39.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 39.6 MPa·√m | T7451 | WL 3.4144-1 | Plate | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 7000 Series Aluminium | ||||
Schubmodule | 26.4 - 27.1 GPa Show Material materials with Schubmodule of 26.4 - 27.1 GPa | Typical for Wrought 7000 Series Aluminium | ||||
Zugfestigkeit | 20.0 °C | 435.0 MPa Show Material materials with Zugfestigkeit of 435.0 MPa | T7451 | WL 3.4144-1 | Plate | Transverse |
20.0 °C | 445.0 MPa Show Material materials with Zugfestigkeit of 445.0 MPa | T7451 | WL 3.4144-1 | Plate | Transverse | |
20.0 °C | 455.0 MPa Show Material materials with Zugfestigkeit of 455.0 MPa | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 460.0 MPa Show Material materials with Zugfestigkeit of 460.0 MPa | T7451 | WL 3.4144-1 | Plate | Transverse | |
20.0 °C | 465.0 MPa Show Material materials with Zugfestigkeit of 465.0 MPa | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 470.0 MPa Show Material materials with Zugfestigkeit of 470.0 MPa | T7451 | WL 3.4144-1 | Plate | Transverse | |
20.0 °C | 475.0 MPa Show Material materials with Zugfestigkeit of 475.0 MPa | T7451 | WL 3.4144-1 | Plate | Transverse | |
20.0 °C | 480.0 MPa Show Material materials with Zugfestigkeit of 480.0 MPa | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 490.0 MPa Show Material materials with Zugfestigkeit of 490.0 MPa | T7451 | WL 3.4144-1 | Plate | Transverse | |
20.0 °C | 490.0 MPa Show Material materials with Zugfestigkeit of 490.0 MPa | T7451 | WL 3.4144-1 | Plate | ||
20.0 °C | 495.0 MPa Show Material materials with Zugfestigkeit of 495.0 MPa | T7451 | WL 3.4144-1 | Plate | Transverse |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100.0 °C | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | T7451 | WL 3.4144-1 | Plate | |
200.0 °C | 2.43e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.43e-05 1/K | T7451 | WL 3.4144-1 | Plate | ||
300.0 °C | 2.52e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.52e-05 1/K | T7451 | WL 3.4144-1 | Plate | ||
Schmelzpunkt | 465.0 - 655.0 °C Show Material materials with Schmelzpunkt of 465.0 - 655.0 °C | Typical for Wrought 7000 Series Aluminium | ||||
Spezifische Wärmekapazität | 100.0 °C | 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 963.0 J/(kg·K) | T7451 | WL 3.4144-1 | Plate | |
Wärmeleitfähigkeit | 25.0 °C | 157.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 157.0 W/(m·K) | T7451 | WL 3.4144-1 | Plate |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 18000000.0 - 34000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 - 34000000.0 S/m | Typical for Wrought 7000 Series Aluminium |
spezifischer Widerstand | 2.9e-08 - 5.6e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.9e-08 - 5.6e-08 Ω·m | Typical for Wrought 7000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.04 Show Material materials with Chrom of 0.04 | T7451 | WL 3.4144-1 | Plate |
Eisen | 0.15 Show Material materials with Eisen of 0.15 | T7451 | WL 3.4144-1 | Plate |
Kupfer | 2.0 - 2.6 % Show Material materials with Kupfer of 2.0 - 2.6 % | T7451 | WL 3.4144-1 | Plate |
Magnesium | 1.9 - 2.6 % Show Material materials with Magnesium of 1.9 - 2.6 % | T7451 | WL 3.4144-1 | Plate |
Mangan | 0.1 Show Material materials with Mangan of 0.1 | T7451 | WL 3.4144-1 | Plate |
Silizium | 0.12 Show Material materials with Silizium of 0.12 | T7451 | WL 3.4144-1 | Plate |
Titan | 0.06 Show Material materials with Titan of 0.06 | T7451 | WL 3.4144-1 | Plate |
Zink | 5.7 - 6.7 % Show Material materials with Zink of 5.7 - 6.7 % | T7451 | WL 3.4144-1 | Plate |
Zirkonium | 0.08 - 0.15 % Show Material materials with Zirkonium of 0.08 - 0.15 % | T7451 | WL 3.4144-1 | Plate |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent |