Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.82 g/cm³ Show Material materials with Dichte of 2.82 g/cm³ | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 8.0 % Show Material materials with Dehnung of 8.0 % | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire | A50 | |
9.0 % Show Material materials with Dehnung of 9.0 % | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire | A50 | ||
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 9.0 % Show Material materials with Dehnung of 9.0 % | T7451 | WL 3.4394 | Plate | ||
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire | ||
Härte, Brinell | 135.0 [-] Show Material materials with Härte, Brinell of 135.0 [-] | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire | ||
20.0 °C | 135.0 [-] Show Material materials with Härte, Brinell of 135.0 [-] | T7451 | WL 3.4394 | Plate | ||
Plane-Strain Fracture Toughnes | 20.0 °C | 24.0 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | |
20.0 °C | 24.0 - 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 24.0 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 24.0 - 33.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 33.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 24.0 - 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 29.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 24.0 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 24.0 - 30.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 30.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 24.0 - 27.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 27.6 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 24.0 - 31.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 31.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 24.0 - 28.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 28.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 24.0 - 33.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 33.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 24.0 - 26.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 24.0 - 26.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 33.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 33.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 29.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 30.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 30.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 27.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 27.6 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 31.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 31.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 28.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 28.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 33.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 33.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.2 - 26.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.2 - 26.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 33.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 33.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 29.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 30.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 30.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 27.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 27.6 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 31.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 31.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 28.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 28.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 - 33.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 - 33.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 26.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 26.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 - 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 - 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 - 33.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 - 33.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 - 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 - 29.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 - 30.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 - 30.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 - 31.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 - 31.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 - 28.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 - 28.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 27.6 - 33.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 27.6 - 33.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 28.1 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.1 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 28.1 - 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.1 - 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 28.1 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.1 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 28.1 - 33.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.1 - 33.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 28.1 - 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.1 - 29.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 28.1 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.1 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 28.1 - 30.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.1 - 30.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 28.1 - 31.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.1 - 31.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 28.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 28.1 - 33.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 28.1 - 33.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 29.0 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 29.0 - 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 29.0 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 29.0 - 33.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 33.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 29.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 29.0 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 29.0 - 30.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 30.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 29.0 - 31.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 31.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 29.0 - 33.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 29.0 - 33.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 30.0 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.0 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 30.0 - 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.0 - 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 30.0 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.0 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 30.0 - 33.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.0 - 33.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 30.0 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.0 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 30.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 30.0 - 31.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.0 - 31.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 30.0 - 33.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 30.0 - 33.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 31.7 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 31.7 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 31.7 - 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 31.7 - 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 31.7 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 31.7 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 31.7 - 33.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 31.7 - 33.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 31.7 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 31.7 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 31.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 31.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 31.7 - 33.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 31.7 - 33.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.0 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.0 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.0 - 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.0 - 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.0 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.0 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.0 - 33.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.0 - 33.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.0 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.0 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.8 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.8 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.8 - 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.8 - 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.8 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.8 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.8 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.8 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 33.8 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 33.8 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 34.1 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 34.1 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 34.1 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 34.1 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 34.1 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 34.1 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 34.1 - 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 34.1 - 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 35.7 - 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 35.7 - 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 35.7 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 35.7 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 35.7 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 35.7 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 39.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 39.0 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 39.0 - 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 39.0 - 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 41.5 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 41.5 MPa·√m | T7451 | WL 3.4394 | Plate | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 7000 Series Aluminium | ||||
Schubmodule | 27.0 GPa Show Material materials with Schubmodule of 27.0 GPa | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire | ||
Zugfestigkeit | 455.0 MPa Show Material materials with Zugfestigkeit of 455.0 MPa | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire | ||
465.0 MPa Show Material materials with Zugfestigkeit of 465.0 MPa | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire | |||
480.0 MPa Show Material materials with Zugfestigkeit of 480.0 MPa | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire | |||
490.0 MPa Show Material materials with Zugfestigkeit of 490.0 MPa | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire | |||
20.0 °C | 455.0 MPa Show Material materials with Zugfestigkeit of 455.0 MPa | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 465.0 MPa Show Material materials with Zugfestigkeit of 465.0 MPa | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 480.0 MPa Show Material materials with Zugfestigkeit of 480.0 MPa | T7451 | WL 3.4394 | Plate | ||
20.0 °C | 490.0 MPa Show Material materials with Zugfestigkeit of 490.0 MPa | T7451 | WL 3.4394 | Plate |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 2.1e-05 - 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1e-05 - 2.4e-05 1/K | Typical for Wrought 7000 Series Aluminium |
Schmelzpunkt | 465.0 - 655.0 °C Show Material materials with Schmelzpunkt of 465.0 - 655.0 °C | Typical for Wrought 7000 Series Aluminium |
Spezifische Wärmekapazität | 795.0 - 1050.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 795.0 - 1050.0 J/(kg·K) | Typical for Wrought 7000 Series Aluminium |
Wärmeleitfähigkeit | 121.0 - 170.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 121.0 - 170.0 W/(m·K) | Typical for Wrought 7000 Series Aluminium |
Elektrisch
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Elektrische Leitfähigkeit | 23000000.0 - 25000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 25000000.0 S/m | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire |
spezifischer Widerstand | 4e-08 - 4.35e-08 Ω·m Show Material materials with spezifischer Widerstand of 4e-08 - 4.35e-08 Ω·m | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.05 % Show Material materials with Chrom of 0.05 % | T7451 | WL 3.4394 | Plate, Sheet, Strip, Bar, Wire |
Eisen | 0.15 % Show Material materials with Eisen of 0.15 % | T7451 | WL 3.4394 | Plate |
0.15 % Show Material materials with Eisen of 0.15 % | T7451 | WL 3.4394 | Sheet, Strip, Bar, Wire | |
Kupfer | 1.5 - 2.0 % Show Material materials with Kupfer of 1.5 - 2.0 % | T7451 | WL 3.4394 | Plate, Sheet, Strip, Bar, Wire |
Magnesium | 2.1 - 2.6 % Show Material materials with Magnesium of 2.1 - 2.6 % | T7451 | WL 3.4394 | Plate, Sheet, Strip, Bar, Wire |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | T7451 | WL 3.4394 | Plate, Sheet, Strip, Bar, Wire |
Nickel | 0.05 % Show Material materials with Nickel of 0.05 % | T7451 | WL 3.4394 | Plate, Sheet, Strip, Bar, Wire |
Silizium | 0.12 % Show Material materials with Silizium of 0.12 % | T7451 | WL 3.4394 | Plate, Sheet, Strip, Bar, Wire |
Titan | 0.06 % Show Material materials with Titan of 0.06 % | T7451 | WL 3.4394 | Plate, Sheet, Strip, Bar, Wire |
Zink | 5.7 - 6.7 % Show Material materials with Zink of 5.7 - 6.7 % | T7451 | WL 3.4394 | Plate, Sheet, Strip, Bar, Wire |
Zirkonium | 0.1 - 0.16 % Show Material materials with Zirkonium of 0.1 - 0.16 % | T7451 | WL 3.4394 | Plate, Sheet, Strip, Bar, Wire |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent |