Allgemein
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 90.0 MPa Show Material materials with Bending Fatigue Strength of 90.0 MPa | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
Biegewinkel 180° | 0.5 °/t Show Material materials with Biegewinkel 180° of 0.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
1.0 °/t Show Material materials with Biegewinkel 180° of 1.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
Biegewinkel 90° | 1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
1.5 °/t Show Material materials with Biegewinkel 90° of 1.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
2.5 °/t Show Material materials with Biegewinkel 90° of 2.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
4.0 °/t Show Material materials with Biegewinkel 90° of 4.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
Dehnung | 10.0 % Show Material materials with Dehnung of 10.0 % | O | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | A50 | |
10.0 % Show Material materials with Dehnung of 10.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | A100 | ||
12.0 % Show Material materials with Dehnung of 12.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | A50 | ||
12.0 % Show Material materials with Dehnung of 12.0 % | O | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | A100 | ||
13.0 % Show Material materials with Dehnung of 13.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | A50 | ||
16.0 % Show Material materials with Dehnung of 16.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | A50 | ||
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | O | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | O | EN 573-3 | Flat | ||
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | O | EN 573-3 | Profile, Rod, Tube | ||
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 13.0 % Show Material materials with Dehnung of 13.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 13.0 % Show Material materials with Dehnung of 13.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | O | EN 573-3 | Flat | A50 Transverse | |
Elastizitätsmodul | 73.0 GPa Show Material materials with Elastizitätsmodul of 73.0 GPa | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
20.0 °C | 72.0 GPa Show Material materials with Elastizitätsmodul of 72.0 GPa | O | EN 573-3 | Profile, Rod, Flat, Tube | ||
Härte, Brinell | 55.0 [-] Show Material materials with Härte, Brinell of 55.0 [-] | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
20.0 °C | 45.0 [-] Show Material materials with Härte, Brinell of 45.0 [-] | O | EN 573-3 | Profile, Rod, Tube | ||
20.0 °C | 55.0 [-] Show Material materials with Härte, Brinell of 55.0 [-] | O | EN 573-3 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Schubmodule | 27.4 GPa Show Material materials with Schubmodule of 27.4 GPa | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
Zugfestigkeit | 220.0 Show Material materials with Zugfestigkeit of 220.0 | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
240.0 Show Material materials with Zugfestigkeit of 240.0 | O | EN 573-3, EN 754 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
250.0 Show Material materials with Zugfestigkeit of 250.0 | O | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
20.0 °C | 220.0 Show Material materials with Zugfestigkeit of 220.0 | O | EN 573-3 | Flat | ||
20.0 °C | 220.0 MPa Show Material materials with Zugfestigkeit of 220.0 MPa | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 235.0 Show Material materials with Zugfestigkeit of 235.0 | O | EN 573-3 | Flat | ||
20.0 °C | 240.0 Show Material materials with Zugfestigkeit of 240.0 | O | EN 573-3 | Rod, Tube | ||
20.0 °C | 250.0 Show Material materials with Zugfestigkeit of 250.0 | O | EN 573-3 | Profile, Rod, Tube |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.1e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | |
-50.0 °C | 2.1e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
20 °C | 2.1e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
20 °C | 2.28e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.28e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
20 °C | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
20 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
20 °C | 2.46e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.46e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
100 °C | 2.28e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.28e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
100.0 °C | 2.28e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.28e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
100 °C | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
200 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
200.0 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
300 °C | 2.46e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.46e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
300.0 °C | 2.46e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.46e-05 1/K | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod, Flat | ||
Schmelzpunkt | 505.0 - 635.0 °C Show Material materials with Schmelzpunkt of 505.0 - 635.0 °C | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
510.0 - 640.0 °C Show Material materials with Schmelzpunkt of 510.0 - 640.0 °C | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
Spezifische Wärmekapazität | 816.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 816.0 - 963.0 J/(kg·K) | Typical for Wrought 2000 Series Aluminium | ||||
Wärmeleitfähigkeit | 134.0 - 193.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 134.0 - 193.0 W/(m·K) | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
20.0 °C | 140.0 - 200.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 140.0 - 200.0 W/(m·K) | O | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Forging, Bar |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 21000000.0 - 24000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 21000000.0 - 24000000.0 S/m | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |
20.0 °C | 20000000.0 - 29000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 20000000.0 - 29000000.0 S/m | O | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Forging, Bar | |
spezifischer Widerstand | 3.45e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.45e-08 - 5e-08 Ω·m | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |
4.17e-08 - 4.76e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.17e-08 - 4.76e-08 Ω·m | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | O | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Forging, Bar |
Eisen | 0.5 % Show Material materials with Eisen of 0.5 % | O | EN 573-3 | Profile, Rod, Flat, Tube |
0.7 % Show Material materials with Eisen of 0.7 % | O | EN 573-3 | Profile, Rod, Flat, Tube | |
0.70 % Show Material materials with Eisen of 0.70 % | O | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |
Kupfer | 3.9 - 5.0 % Show Material materials with Kupfer of 3.9 - 5.0 % | O | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Forging, Bar |
Magnesium | 0.2 - 0.8 % Show Material materials with Magnesium of 0.2 - 0.8 % | O | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Forging, Bar |
Mangan | 0.4 - 1.2 % Show Material materials with Mangan of 0.4 - 1.2 % | O | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Forging, Bar |
Nickel | 0.1 Show Material materials with Nickel of 0.1 | O | EN 573-3 | Profile, Rod, Flat, Tube |
Silizium | 0.5 - 1.2 % Show Material materials with Silizium of 0.5 - 1.2 % | O | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Forging, Bar |
0.5 - 0.9 % Show Material materials with Silizium of 0.5 - 0.9 % | O | EN 573-3 | Profile, Rod, Flat, Tube | |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | O | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Forging, Bar |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | O | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Forging, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not suitable, Protective: acceptable | |
Brazing | hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable | |
Corrosion properties | Seawater: sufficient, weathering: acceptable | |
Workability | Bending / Spinning (cold): gut (O) / ungeeignet, Impact extrusion (cold): not suitable, Deep drawing / upsetting (Condition) acceptable (O) / not suitable |