Allgemein
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 4.0 % Show Material materials with Dehnung of 4.0 % | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | A50 | |
5.0 % Show Material materials with Dehnung of 5.0 % | T6510 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | A50 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | T6510 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | A100 | ||
6.0 % Show Material materials with Dehnung of 6.0 % | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | A100 | ||
7.0 % Show Material materials with Dehnung of 7.0 % | T6510 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | A100 | ||
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | T6510 | EN 573-3 | Tube | A50 | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | T6510 | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | T6510 | EN 573-3 | Rod | ||
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | T6510 | EN 573-3 | Tube, Rod | ||
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | T6510 | EN 573-3 | Profile, Rod, Tube | ||
Elastizitätsmodul | 73.0 GPa Show Material materials with Elastizitätsmodul of 73.0 GPa | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
20.0 °C | 72.0 GPa Show Material materials with Elastizitätsmodul of 72.0 GPa | T6510 | EN 573-3 | Profile, Rod, Tube | ||
Härte, Brinell | 20.0 °C | 140.0 [-] Show Material materials with Härte, Brinell of 140.0 [-] | T6510 | EN 573-3 | Profile, Rod, Tube | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Schubmodule | 27.4 GPa Show Material materials with Schubmodule of 27.4 GPa | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
Zugfestigkeit | 415.0 MPa Show Material materials with Zugfestigkeit of 415.0 MPa | T6510 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
420.0 MPa Show Material materials with Zugfestigkeit of 420.0 MPa | T6510 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
430.0 MPa Show Material materials with Zugfestigkeit of 430.0 MPa | T6510 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
450.0 MPa Show Material materials with Zugfestigkeit of 450.0 MPa | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
460.0 MPa Show Material materials with Zugfestigkeit of 460.0 MPa | T6510 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
465.0 MPa Show Material materials with Zugfestigkeit of 465.0 MPa | T6510 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
20.0 °C | 415.0 MPa Show Material materials with Zugfestigkeit of 415.0 MPa | T6510 | EN 573-3 | Tube, Profile, Rod | ||
20.0 °C | 420.0 MPa Show Material materials with Zugfestigkeit of 420.0 MPa | T6510 | EN 573-3 | Rod | ||
20.0 °C | 430.0 MPa Show Material materials with Zugfestigkeit of 430.0 MPa | T6510 | EN 573-3 | Rod | ||
20.0 °C | 450.0 MPa Show Material materials with Zugfestigkeit of 450.0 MPa | T6510 | EN 573-3 | Tube | ||
20.0 °C | 460.0 MPa Show Material materials with Zugfestigkeit of 460.0 MPa | T6510 | EN 573-3 | Profile, Rod | ||
20.0 °C | 465.0 MPa Show Material materials with Zugfestigkeit of 465.0 MPa | T6510 | EN 573-3 | Rod |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.1e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1e-05 1/K | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod | |
-50.0 °C | 2.1e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1e-05 1/K | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod | ||
20 °C | 2.1e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1e-05 1/K | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod | ||
20 °C | 2.28e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.28e-05 1/K | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod | ||
20 °C | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
20 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod | ||
20 °C | 2.46e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.46e-05 1/K | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod | ||
100 °C | 2.28e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.28e-05 1/K | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod | ||
100.0 °C | 2.28e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.28e-05 1/K | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod | ||
100 °C | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
200 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod | ||
200.0 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod | ||
300 °C | 2.46e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.46e-05 1/K | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod | ||
300.0 °C | 2.46e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.46e-05 1/K | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar, Profile, Rod | ||
Schmelzpunkt | 505.0 - 635.0 °C Show Material materials with Schmelzpunkt of 505.0 - 635.0 °C | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
510.0 - 640.0 °C Show Material materials with Schmelzpunkt of 510.0 - 640.0 °C | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |||
Spezifische Wärmekapazität | 816.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 816.0 - 963.0 J/(kg·K) | Typical for Wrought 2000 Series Aluminium | ||||
Wärmeleitfähigkeit | 134.0 - 193.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 134.0 - 193.0 W/(m·K) | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | ||
20.0 °C | 140.0 - 200.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 140.0 - 200.0 W/(m·K) | T6510 | EN 573-3, EN 754, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate, Forging, Bar |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 21000000.0 - 24000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 21000000.0 - 24000000.0 S/m | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |
20.0 °C | 20000000.0 - 29000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 20000000.0 - 29000000.0 S/m | T6510 | EN 573-3, EN 754, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate, Forging, Bar | |
spezifischer Widerstand | 3.45e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.45e-08 - 5e-08 Ω·m | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |
4.17e-08 - 4.76e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.17e-08 - 4.76e-08 Ω·m | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | T6510 | EN 573-3, EN 754, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate, Forging, Bar |
Eisen | 0.5 % Show Material materials with Eisen of 0.5 % | T6510 | EN 573-3 | Profile, Rod, Tube |
0.7 % Show Material materials with Eisen of 0.7 % | T6510 | EN 573-3 | Profile, Rod, Tube | |
0.70 % Show Material materials with Eisen of 0.70 % | T6510 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Bar | |
Kupfer | 3.9 - 5.0 % Show Material materials with Kupfer of 3.9 - 5.0 % | T6510 | EN 573-3, EN 754, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate, Forging, Bar |
Magnesium | 0.2 - 0.8 % Show Material materials with Magnesium of 0.2 - 0.8 % | T6510 | EN 573-3, EN 754, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate, Forging, Bar |
Mangan | 0.4 - 1.2 % Show Material materials with Mangan of 0.4 - 1.2 % | T6510 | EN 573-3, EN 754, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate, Forging, Bar |
Nickel | 0.1 Show Material materials with Nickel of 0.1 | T6510 | EN 573-3 | Profile, Rod, Tube |
Silizium | 0.5 - 1.2 % Show Material materials with Silizium of 0.5 - 1.2 % | T6510 | EN 573-3, EN 754, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate, Forging, Bar |
0.5 - 0.9 % Show Material materials with Silizium of 0.5 - 0.9 % | T6510 | EN 573-3 | Profile, Rod, Tube | |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | T6510 | EN 573-3, EN 754, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate, Forging, Bar |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | T6510 | EN 573-3, EN 754, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate, Forging, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not suitable, Protective: acceptable | |
Brazing | hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable | |
Corrosion properties | Seawater: sufficient, weathering: acceptable | |
Workability | Bending / Spinning (cold): gut (O) / ungeeignet, Impact extrusion (cold): not suitable, Deep drawing / upsetting (Condition) acceptable (O) / not suitable |