Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.8 g/cm³ Show Material materials with Dichte of 2.8 g/cm³ | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Biegewinkel 90° | 5.0 °/t Show Material materials with Biegewinkel 90° of 5.0 °/t | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
6.0 °/t Show Material materials with Biegewinkel 90° of 6.0 °/t | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
Dehnung | 4.0 % Show Material materials with Dehnung of 4.0 % | T651 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | |
4.0 % Show Material materials with Dehnung of 4.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
6.0 % Show Material materials with Dehnung of 6.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
6.0 % Show Material materials with Dehnung of 6.0 % | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
7.0 % Show Material materials with Dehnung of 7.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
8.0 % Show Material materials with Dehnung of 8.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | T651 | EN 573-3 | Rod | A50 | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | T651 | EN 573-3 | Flat | ||
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | T651 | EN 573-3 | Flat | ||
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | T651 | EN 573-3 | Flat | A50 | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | T651 | EN 573-3 | Rod, Flat | ||
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | T651 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | T651 | EN 573-3 | Flat | A50 | |
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | T651 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | T651 | EN 573-3 | Flat | A50 | |
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | T651 | EN 573-3 | Flat | A50 Transverse | |
Elastizitätsmodul | 73.0 GPa Show Material materials with Elastizitätsmodul of 73.0 GPa | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
Härte, Brinell | 150.0 [-] Show Material materials with Härte, Brinell of 150.0 [-] | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 140.0 [-] Show Material materials with Härte, Brinell of 140.0 [-] | T651 | EN 573-3 | Rod | ||
20.0 °C | 150.0 [-] Show Material materials with Härte, Brinell of 150.0 [-] | T651 | EN 573-3 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Schubmodule | 27.4 GPa Show Material materials with Schubmodule of 27.4 GPa | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
Zugfestigkeit | 410.0 MPa Show Material materials with Zugfestigkeit of 410.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
420.0 MPa Show Material materials with Zugfestigkeit of 420.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
430.0 MPa Show Material materials with Zugfestigkeit of 430.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
440.0 MPa Show Material materials with Zugfestigkeit of 440.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
450.0 MPa Show Material materials with Zugfestigkeit of 450.0 MPa | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
460.0 MPa Show Material materials with Zugfestigkeit of 460.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
20.0 °C | 410.0 MPa Show Material materials with Zugfestigkeit of 410.0 MPa | T651 | EN 573-3 | Flat | ||
20.0 °C | 420.0 MPa Show Material materials with Zugfestigkeit of 420.0 MPa | T651 | EN 573-3 | Flat | ||
20.0 °C | 420.0 MPa Show Material materials with Zugfestigkeit of 420.0 MPa | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 430.0 MPa Show Material materials with Zugfestigkeit of 430.0 MPa | T651 | EN 573-3 | Flat | ||
20.0 °C | 430.0 MPa Show Material materials with Zugfestigkeit of 430.0 MPa | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 440.0 MPa Show Material materials with Zugfestigkeit of 440.0 MPa | T651 | EN 573-3 | Flat | ||
20.0 °C | 440.0 MPa Show Material materials with Zugfestigkeit of 440.0 MPa | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 450.0 MPa Show Material materials with Zugfestigkeit of 450.0 MPa | T651 | EN 573-3 | Rod, Flat | ||
20.0 °C | 450.0 MPa Show Material materials with Zugfestigkeit of 450.0 MPa | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 460.0 MPa Show Material materials with Zugfestigkeit of 460.0 MPa | T651 | EN 573-3 | Flat | ||
20.0 °C | 460.0 MPa Show Material materials with Zugfestigkeit of 460.0 MPa | T651 | EN 573-3 | Flat | Transverse |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 1.6e-05 - 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6e-05 - 2.4e-05 1/K | Typical for Wrought 2000 Series Aluminium |
Schmelzpunkt | 500.0 - 650.0 °C Show Material materials with Schmelzpunkt of 500.0 - 650.0 °C | Typical for Wrought 2000 Series Aluminium |
Spezifische Wärmekapazität | 816.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 816.0 - 963.0 J/(kg·K) | Typical for Wrought 2000 Series Aluminium |
Wärmeleitfähigkeit | 112.0 - 251.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 112.0 - 251.0 W/(m·K) | Typical for Wrought 2000 Series Aluminium |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 18000000.0 - 30000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 - 30000000.0 S/m | Typical for Wrought 2000 Series Aluminium |
spezifischer Widerstand | 3.4e-08 - 6e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.4e-08 - 6e-08 Ω·m | Typical for Wrought 2000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Beryllium | 0.0001 - 0.005 % Show Material materials with Beryllium of 0.0001 - 0.005 % | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | T651 | EN 573-3, EN 485, EN 754 | Rod, Flat, Strip, Sheet, Plate, Welded Tube, Tube, Wire |
Eisen | 0.5 % Show Material materials with Eisen of 0.5 % | T651 | EN 573-3 | Rod, Flat |
0.50 % Show Material materials with Eisen of 0.50 % | T651 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |
Kupfer | 3.9 - 5.0 % Show Material materials with Kupfer of 3.9 - 5.0 % | T651 | EN 573-3, EN 485, EN 754 | Rod, Flat, Strip, Sheet, Plate, Welded Tube, Tube, Wire |
Magnesium | 0.2 - 0.8 % Show Material materials with Magnesium of 0.2 - 0.8 % | T651 | EN 573-3, EN 485, EN 754 | Rod, Flat, Strip, Sheet, Plate, Welded Tube, Tube, Wire |
Mangan | 0.4 - 1.2 % Show Material materials with Mangan of 0.4 - 1.2 % | T651 | EN 573-3, EN 485, EN 754 | Rod, Flat, Strip, Sheet, Plate, Welded Tube, Tube, Wire |
Nickel | 0.1 % Show Material materials with Nickel of 0.1 % | T651 | EN 573-3, EN 485, EN 754 | Rod, Flat, Strip, Sheet, Plate, Welded Tube, Tube, Wire |
Silizium | 0.5 - 0.9 % Show Material materials with Silizium of 0.5 - 0.9 % | T651 | EN 573-3, EN 485, EN 754 | Rod, Flat, Strip, Sheet, Plate, Welded Tube, Tube, Wire |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | T651 | EN 573-3, EN 485, EN 754 | Rod, Flat, Strip, Sheet, Plate, Welded Tube, Tube, Wire |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | T651 | EN 573-3, EN 485, EN 754 | Rod, Flat, Strip, Sheet, Plate, Welded Tube, Tube, Wire |
Technological properties
Property | ||
---|---|---|
Workability | Moderate Workability |