Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20.0 °C | 2.77 g/cm³ Show Material materials with Dichte of 2.77 g/cm³ | T4510 | EN 573-3 | Rod |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | T4510 | EN 573-3 | Rod | |
Elastizitätsmodul | 20.0 °C | 70.0 - 74.5 GPa Show Material materials with Elastizitätsmodul of 70.0 - 74.5 GPa | T4510 | EN 573-3 | Rod | |
Härte, Brinell | 20.0 °C | 110.0 [-] Show Material materials with Härte, Brinell of 110.0 [-] | T4510 | EN 573-3 | Rod | |
20.0 °C | 110.0 - 138.0 [-] Show Material materials with Härte, Brinell of 110.0 - 138.0 [-] | T4510 | EN 573-3 | Rod | ||
20.0 °C | 138.0 [-] Show Material materials with Härte, Brinell of 138.0 [-] | T4510 | EN 573-3 | Rod | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Schubmodule | 20.0 °C | 27.0 - 28.0 GPa Show Material materials with Schubmodule of 27.0 - 28.0 GPa | T4510 | EN 573-3 | Rod | |
Zugfestigkeit | 20.0 °C | 360.0 MPa Show Material materials with Zugfestigkeit of 360.0 MPa | T4510 | EN 573-3 | Rod |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 1.6e-05 - 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6e-05 - 2.4e-05 1/K | Typical for Wrought 2000 Series Aluminium | ||||
Schmelzpunkt | 500.0 - 650.0 °C Show Material materials with Schmelzpunkt of 500.0 - 650.0 °C | Typical for Wrought 2000 Series Aluminium | ||||
Spezifische Wärmekapazität | 20.0 °C | 875.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 875.0 J/(kg·K) | T4510 | EN 573-3 | Rod | |
Wärmeleitfähigkeit | 20.0 °C | 130.0 - 150.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 150.0 W/(m·K) | T4510 | EN 573-3 | Rod |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 18000000.0 - 21000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 - 21000000.0 S/m | T4510 | EN 573-3 | Rod | |
spezifischer Widerstand | 3.4e-08 - 6e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.4e-08 - 6e-08 Ω·m | Typical for Wrought 2000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.1 Show Material materials with Chrom of 0.1 | T4510 | EN 573-3 | Rod |
Eisen | 0.5 Show Material materials with Eisen of 0.5 | T4510 | EN 573-3 | Rod |
Kupfer | 3.8 - 4.9 % Show Material materials with Kupfer of 3.8 - 4.9 % | T4510 | EN 573-3 | Rod |
Magnesium | 1.2 - 1.8 % Show Material materials with Magnesium of 1.2 - 1.8 % | T4510 | EN 573-3 | Rod |
Mangan | 0.3 - 0.9 % Show Material materials with Mangan of 0.3 - 0.9 % | T4510 | EN 573-3 | Rod |
Silizium | 0.5 Show Material materials with Silizium of 0.5 | T4510 | EN 573-3 | Rod |
Titan | 0.15 Show Material materials with Titan of 0.15 | T4510 | EN 573-3 | Rod |
Zink | 0.25 Show Material materials with Zink of 0.25 | T4510 | EN 573-3 | Rod |
Technological properties
Property | ||
---|---|---|
Workability | Moderate Workability |