Allgemein
Property | Value | Related Standards | Shape |
---|---|---|---|
Dichte | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | EN 573-3 | Strip, Sheet, Plate, Tube, Bar |
Mechanisch
Property | Value | Related Standards | Shape | Comment |
---|---|---|---|---|
Elastizitätsmodul | 79.0 GPa Show Material materials with Elastizitätsmodul of 79.0 GPa | EN 573-3 | Strip, Sheet, Plate, Tube, Bar | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 4000 Series Aluminium | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 4000 Series Aluminium | ||
Schubmodule | 26.0 GPa Show Material materials with Schubmodule of 26.0 GPa | Typical for Wrought 4000 Series Aluminium |
Thermisch
Property | Temperature | Value | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 1.9399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.9399999999999997e-05 1/K | EN 573-3 | Strip, Sheet, Plate, Tube, Bar | |
100 °C | 1.9399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.9399999999999997e-05 1/K | EN 573-3 | Strip, Sheet, Plate, Tube, Bar | ||
Schmelzpunkt | 530.0 - 570.0 °C Show Material materials with Schmelzpunkt of 530.0 - 570.0 °C | EN 573-3 | Strip, Sheet, Plate, Tube, Bar | ||
Spezifische Wärmekapazität | 864.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 864.0 J/(kg·K) | Typical for Wrought 4000 Series Aluminium | |||
Wärmeleitfähigkeit | 138.0 - 155.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 138.0 - 155.0 W/(m·K) | EN 573-3 | Strip, Sheet, Plate, Tube, Bar |
Elektrisch
Property | Value | Related Standards | Shape |
---|---|---|---|
Elektrische Leitfähigkeit | 20000000.0 - 23000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 20000000.0 - 23000000.0 S/m | EN 573-3 | Strip, Sheet, Plate, Tube, Bar |
spezifischer Widerstand | 4.35e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.35e-08 - 5e-08 Ω·m | EN 573-3 | Strip, Sheet, Plate, Tube, Bar |
Chemical properties
Property | Value | Related Standards | Shape |
---|---|---|---|
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | EN 573-3 | Strip, Sheet, Plate, Tube, Bar |
Eisen | 1.0 % Show Material materials with Eisen of 1.0 % | EN 573-3 | |
1.00 % Show Material materials with Eisen of 1.00 % | EN 573-3 | Strip, Sheet, Plate, Tube, Bar | |
Kupfer | 0.5 - 1.3 % Show Material materials with Kupfer of 0.5 - 1.3 % | EN 573-3 | Strip, Sheet, Plate, Tube, Bar |
Magnesium | 0.8 - 1.3 % Show Material materials with Magnesium of 0.8 - 1.3 % | EN 573-3 | Strip, Sheet, Plate, Tube, Bar |
Nickel | 0.5 - 1.3 % Show Material materials with Nickel of 0.5 - 1.3 % | EN 573-3 | Strip, Sheet, Plate, Tube, Bar |
Silizium | 11.0 - 13.5 % Show Material materials with Silizium of 11.0 - 13.5 % | EN 573-3 | Strip, Sheet, Plate, Tube, Bar |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | EN 573-3 | Strip, Sheet, Plate, Tube, Bar |
Technological properties
Property | ||
---|---|---|
Workability | Moderate Workability |