Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod |
2.705 g/cm³ Show Material materials with Dichte of 2.705 g/cm³ | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 20.0 % Show Material materials with Dehnung of 20.0 % | H112 | EN 573-3, EN 485 | Plate, Rod | A50 | |
20.0 % Show Material materials with Dehnung of 20.0 % | H112 | EN 573-3, EN 485 | Plate, Rod | |||
23.0 % Show Material materials with Dehnung of 23.0 % | H112 | EN 573-3, EN 755 | Plate, Rod | A50 | ||
25.0 % Show Material materials with Dehnung of 25.0 % | H112 | EN 573-3, EN 755 | Plate, Rod | A100 | ||
20.0 °C | 23.0 % Show Material materials with Dehnung of 23.0 % | H112 | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 25.0 % Show Material materials with Dehnung of 25.0 % | H112 | EN 573-3 | Profile, Rod, Tube | ||
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod | ||
70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod | |||
Härte, Brinell | 23.0 [-] Show Material materials with Härte, Brinell of 23.0 [-] | H112 | EN 573-3, EN 485 | Plate, Rod | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||||
Schubmodule | 25.9 GPa Show Material materials with Schubmodule of 25.9 GPa | Typical for Wrought 1000 Series Aluminium | ||||
Zugfestigkeit | 60.0 MPa Show Material materials with Zugfestigkeit of 60.0 MPa | H112 | EN 573-3, EN 755 | Plate, Rod | ||
75.0 MPa Show Material materials with Zugfestigkeit of 75.0 MPa | H112 | EN 573-3, EN 485 | Plate, Rod | |||
20.0 °C | 60.0 MPa Show Material materials with Zugfestigkeit of 60.0 MPa | H112 | EN 573-3 | Profile, Rod, Tube |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod | |
20 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod | ||
100 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod | ||
100 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod | ||
Schmelzpunkt | 645.0 - 657.0 °C Show Material materials with Schmelzpunkt of 645.0 - 657.0 °C | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod | ||
645.0 - 655.0 °C Show Material materials with Schmelzpunkt of 645.0 - 655.0 °C | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod | |||
Spezifische Wärmekapazität | 900.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 - 963.0 J/(kg·K) | Typical for Wrought 1000 Series Aluminium | ||||
Wärmeleitfähigkeit | 225.0 - 235.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 225.0 - 235.0 W/(m·K) | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod | ||
234 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 234 W/(m·K) | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod |
Elektrisch
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Elektrische Leitfähigkeit | 35400000.0 - 36500000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 35400000.0 - 36500000.0 S/m | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod |
36000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 36000000.0 S/m | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod | |
spezifischer Widerstand | 2.74e-08 - 2.82e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.74e-08 - 2.82e-08 Ω·m | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod |
2.78e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.78e-08 Ω·m | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 99.5 % Show Material materials with Aluminium of 99.5 % | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod |
Bor | 0.05 % Show Material materials with Bor of 0.05 % | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod, Profile, Tube |
Chrom | 0.01 % Show Material materials with Chrom of 0.01 % | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod, Profile, Tube |
Eisen | 0.40 % Show Material materials with Eisen of 0.40 % | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod |
0.4 % Show Material materials with Eisen of 0.4 % | H112 | EN 573-3 | Profile, Rod, Tube | |
Gallium | 0.03 % Show Material materials with Gallium of 0.03 % | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod, Profile, Tube |
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod, Profile, Tube |
Mangan | 0.01 % Show Material materials with Mangan of 0.01 % | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod, Profile, Tube |
Silizium | 0.1 % Show Material materials with Silizium of 0.1 % | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod, Profile, Tube |
Zink | 0.05 % Show Material materials with Zink of 0.05 % | H112 | EN 573-3, EN 485, EN 755 | Plate, Rod, Profile, Tube |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent | |
Workability | Excellent workability. |