Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 20.0 °C | 4.505 g/cm³ Show Material materials with Dichte of 4.505 g/cm³ | Annealed | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Bar, Flat, Sheet |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7064-1, VdTÜV WB 230-1, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | Transverse |
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | Annealed | WL 3.7064-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | ||
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7064-1, VdTÜV WB 230-1, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Wire, Sheet | ||
Elastizitätsmodul | 20.0 °C | 108.0 GPa Show Material materials with Elastizitätsmodul of 108.0 GPa | Annealed | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Bar, Flat, Sheet | |
200.0 °C | 95.0 GPa Show Material materials with Elastizitätsmodul of 95.0 GPa | Annealed | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Bar, Flat, Sheet | ||
400.0 °C | 81.0 GPa Show Material materials with Elastizitätsmodul of 81.0 GPa | Annealed | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Bar, Flat, Sheet | ||
Flächenreduzierung | 20.0 °C | 25.0 % Show Material materials with Flächenreduzierung of 25.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7064-1, VdTÜV WB 230-1, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | Transverse |
20.0 °C | 25.0 % Show Material materials with Flächenreduzierung of 25.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7064-1, VdTÜV WB 230-1, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | ||
Härte, Brinell | 20.0 °C | 200.0 Show Material materials with Härte, Brinell of 200.0 | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7064-1, VdTÜV WB 230-1, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | |
20.0 °C | 200.0 Show Material materials with Härte, Brinell of 200.0 | Annealed | DIN 17850, DIN 17864, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17860 | Forging | Transverse | |
Poissonzahl | 0.361 [-] Show Material materials with Poissonzahl of 0.361 [-] | Typical for Pure Titanium | ||||
Schubmodule | 20.0 °C | 45.0 GPa Show Material materials with Schubmodule of 45.0 GPa | Annealed | WL 3.7064-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Sheet | |
Zugfestigkeit | 20.0 °C | 540.0 - 740.0 MPa Show Material materials with Zugfestigkeit of 540.0 - 740.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7064-1, VdTÜV WB 230-1, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Wire | |
20.0 °C | 540.0 - 740.0 MPa Show Material materials with Zugfestigkeit of 540.0 - 740.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7064-1, VdTÜV WB 230-1, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | Transverse | |
20.0 °C | 570.0 - 730.0 MPa Show Material materials with Zugfestigkeit of 570.0 - 730.0 MPa | Annealed | WL 3.7064-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Sheet | ||
20.0 °C | 640.0 MPa Show Material materials with Zugfestigkeit of 640.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7064-1, VdTÜV WB 230-1, DIN 17862, DIN 17864, DIN 17860 | |||
100.0 °C | 540.0 MPa Show Material materials with Zugfestigkeit of 540.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7064-1, VdTÜV WB 230-1, DIN 17862, DIN 17864, DIN 17860 | |||
200.0 °C | 390.0 MPa Show Material materials with Zugfestigkeit of 390.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7064-1, VdTÜV WB 230-1, DIN 17862, DIN 17864, DIN 17860 | |||
300.0 °C | 280.0 MPa Show Material materials with Zugfestigkeit of 280.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, WL 3.7064-1, VdTÜV WB 230-1, DIN 17862, DIN 17864, DIN 17860 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 8.400000000000001e-06 - 8.599999999999999e-06 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 8.400000000000001e-06 - 8.599999999999999e-06 1/K | Typical for Pure Titanium | ||||
Schmelzpunkt | 1670.0 °C Show Material materials with Schmelzpunkt of 1670.0 °C | Typical for Pure Titanium | ||||
Spezifische Wärmekapazität | 20.0 °C | 540.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 540.0 J/(kg·K) | Annealed | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Bar, Flat, Sheet | |
200.0 °C | 570.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 570.0 J/(kg·K) | Annealed | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Bar, Flat, Sheet | ||
400.0 °C | 630.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 630.0 J/(kg·K) | Annealed | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Bar, Flat, Sheet | ||
Wärmeleitfähigkeit | 20.0 °C | 20.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 20.1 W/(m·K) | Annealed | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Bar, Flat, Sheet | |
200.0 °C | 20.1 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 20.1 W/(m·K) | Annealed | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Bar, Flat, Sheet | ||
400.0 °C | 20.5 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 20.5 W/(m·K) | Annealed | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Bar, Flat, Sheet |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
spezifischer Widerstand | 20.0 °C | 5.5e-07 Ω·m Show Material materials with spezifischer Widerstand of 5.5e-07 Ω·m | Annealed | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Bar, Flat, Sheet |
200.0 °C | 8.8e-07 Ω·m Show Material materials with spezifischer Widerstand of 8.8e-07 Ω·m | Annealed | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Bar, Flat, Sheet | |
400.0 °C | 1.22e-06 Ω·m Show Material materials with spezifischer Widerstand of 1.22e-06 Ω·m | Annealed | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Bar, Flat, Sheet |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Eisen | 0.3 Show Material materials with Eisen of 0.3 | Annealed | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Bar, Flat |
0.35 Show Material materials with Eisen of 0.35 | Annealed | WL 3.7064-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Sheet | |
Kohlenstoff | 0.06 Show Material materials with Kohlenstoff of 0.06 | Annealed | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Bar, Flat |
0.08 Show Material materials with Kohlenstoff of 0.08 | Annealed | WL 3.7064-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Sheet | |
Sauerstoff | 0.35 Show Material materials with Sauerstoff of 0.35 | Annealed | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Bar, Flat |
0.4 Show Material materials with Sauerstoff of 0.4 | Annealed | WL 3.7064-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Sheet | |
Stickstoff | 0.05 Show Material materials with Stickstoff of 0.05 | Annealed | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Bar, Flat |
0.07 Show Material materials with Stickstoff of 0.07 | Annealed | WL 3.7064-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Sheet | |
Titan | 98.5 % Show Material materials with Titan of 98.5 % | Annealed | WL 3.7064-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Sheet |
98.8 % Show Material materials with Titan of 98.8 % | Annealed | DIN 17850, DIN 17864, WL 3.7064-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17860 | Forging, Rod, Wire, Flat | |
Wasserstoff | 0.013 Show Material materials with Wasserstoff of 0.013 | Annealed | VdTÜV WB 230-3, WL 3.7064-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1 | Forging, Rod, Wire, Bar, Flat, Sheet |