Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 4.506 g/cm³ Show Material materials with Dichte of 4.506 g/cm³ | Typical for Titanium |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Dehnung | 20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | As-Cast | DIN 17865 | |
Elastizitätsmodul | 100.0 - 120.0 GPa Show Material materials with Elastizitätsmodul of 100.0 - 120.0 GPa | Typical for Titanium Near Alpha Alloy | |||
Zugfestigkeit | 20.0 °C | 450.0 MPa Show Material materials with Zugfestigkeit of 450.0 MPa | As-Cast | DIN 17865 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 7.599999999999997e-06 - 1.1e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 7.599999999999997e-06 - 1.1e-05 1/K | Typical for Titanium Near Alpha Alloy | |||
Schmelzpunkt | 1540.0 - 1715.0 °C Show Material materials with Schmelzpunkt of 1540.0 - 1715.0 °C | Typical for Titanium Near Alpha Alloy | |||
Spezifische Wärmekapazität | 460.0 - 527.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 460.0 - 527.0 J/(kg·K) | Typical for Titanium Near Alpha Alloy | |||
Wärmeleitfähigkeit | 20.0 °C | 16.3 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 16.3 W/(m·K) | As-Cast | DIN 17865 |
Elektrisch
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 1750000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 1750000.0 S/m | As-Cast | DIN 17865 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Eisen | 0.25 Show Material materials with Eisen of 0.25 | As-Cast | DIN 17865 |
Kohlenstoff | 0.1 Show Material materials with Kohlenstoff of 0.1 | As-Cast | DIN 17865 |
Sauerstoff | 0.4 Show Material materials with Sauerstoff of 0.4 | As-Cast | DIN 17865 |
Stickstoff | 0.05 Show Material materials with Stickstoff of 0.05 | As-Cast | DIN 17865 |
Wasserstoff | 0.015 Show Material materials with Wasserstoff of 0.015 | As-Cast | DIN 17865 |
Technological properties
Property | ||
---|---|---|
Processing methods | investment casting, compact casting, separately cast test samples or taken from casting without ingate |