Allgemein
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Dichte | 20.0 °C | 2.75 g/cm³ Show Material materials with Dichte of 2.75 g/cm³ | T5 | DIN 1725-2, EN 1676, EN 1706 |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Dehnung | 220.0 °C | 8.4 % Show Material materials with Dehnung of 8.4 % | T5 | DIN 1725-2, EN 1676, EN 1706 | |
280.0 °C | 21.8 % Show Material materials with Dehnung of 21.8 % | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
Elastizitätsmodul | 20.0 °C | 75.0 GPa Show Material materials with Elastizitätsmodul of 75.0 GPa | T5 | DIN 1725-2, EN 1676, EN 1706 | |
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | |||
Schubmodule | 2.8 GPa Show Material materials with Schubmodule of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | |||
Zugfestigkeit | 20.0 °C | 348.0 MPa Show Material materials with Zugfestigkeit of 348.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | |
220.0 °C | 133.0 MPa Show Material materials with Zugfestigkeit of 133.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
280.0 °C | 66.0 MPa Show Material materials with Zugfestigkeit of 66.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 200.0 °C | 2.1e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1e-05 1/K | T5 | DIN 1725-2, EN 1676, EN 1706 | |
Schmelzpunkt | 505.0 - 770.0 °C Show Material materials with Schmelzpunkt of 505.0 - 770.0 °C | Typical for Cast 3xx.x Series Aluminium | |||
Spezifische Wärmekapazität | 20.0 °C | 880.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 880.0 J/(kg·K) | T5 | DIN 1725-2, EN 1676, EN 1706 | |
Wärmeleitfähigkeit | 20.0 °C | 110.0 - 130.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 110.0 - 130.0 W/(m·K) | T5 | DIN 1725-2, EN 1676, EN 1706 |
Elektrisch
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 14000000.0 - 18000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 14000000.0 - 18000000.0 S/m | T5 | DIN 1725-2, EN 1676, EN 1706 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 82.1 % Show Material materials with Aluminium of 82.1 % | T5 | DIN 1725-2, EN 1676, EN 1706 |
Blei | 0.2 Show Material materials with Blei of 0.2 | T5 | DIN 1725-2, EN 1676, EN 1706 |
Eisen | 0.8 Show Material materials with Eisen of 0.8 | T5 | DIN 1725-2, EN 1676, EN 1706 |
Kupfer | 2.0 - 3.5 % Show Material materials with Kupfer of 2.0 - 3.5 % | T5 | DIN 1725-2, EN 1676, EN 1706 |
Mangan | 0.1 - 0.5 % Show Material materials with Mangan of 0.1 - 0.5 % | T5 | DIN 1725-2, EN 1676, EN 1706 |
Nickel | 0.3 Show Material materials with Nickel of 0.3 | T5 | DIN 1725-2, EN 1676, EN 1706 |
Silizium | 8.0 - 11.0 % Show Material materials with Silizium of 8.0 - 11.0 % | T5 | DIN 1725-2, EN 1676, EN 1706 |
Titan | 0.15 Show Material materials with Titan of 0.15 | T5 | DIN 1725-2, EN 1676, EN 1706 |
Zink | 1.2 Show Material materials with Zink of 1.2 | T5 | DIN 1725-2, EN 1676, EN 1706 |
Zinn | 0.1 Show Material materials with Zinn of 0.1 | T5 | DIN 1725-2, EN 1676, EN 1706 |
Technological properties
Property | ||
---|---|---|
Processing methods | permanent mould casting |