Allgemein
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Dichte | 20.0 °C | 2.65 g/cm³ Show Material materials with Dichte of 2.65 g/cm³ | T5 | DIN 1725-2, EN 1676, EN 1706 |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Dehnung | -196.0 °C | 0.6 % Show Material materials with Dehnung of 0.6 % | T5 | DIN 1725-2, EN 1676, EN 1706 | |
-196.0 °C | 2.4 % Show Material materials with Dehnung of 2.4 % | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
-120.0 °C | 0.5 % Show Material materials with Dehnung of 0.5 % | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
-120.0 °C | 2.4 % Show Material materials with Dehnung of 2.4 % | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
-50.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
-50.0 °C | 2.4 % Show Material materials with Dehnung of 2.4 % | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 0.8 % Show Material materials with Dehnung of 0.8 % | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 1.0 - 4.0 % Show Material materials with Dehnung of 1.0 - 4.0 % | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 2.2 % Show Material materials with Dehnung of 2.2 % | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 2.2 - 2.4 % Show Material materials with Dehnung of 2.2 - 2.4 % | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 2.4 % Show Material materials with Dehnung of 2.4 % | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
220.0 °C | 10.6 % Show Material materials with Dehnung of 10.6 % | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
220.0 °C | 28.4 % Show Material materials with Dehnung of 28.4 % | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
280.0 °C | 30.1 % Show Material materials with Dehnung of 30.1 % | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
Elastizitätsmodul | 20.0 °C | 74.0 GPa Show Material materials with Elastizitätsmodul of 74.0 GPa | T5 | DIN 1725-2, EN 1676, EN 1706 | |
Härte, Brinell | 20.0 °C | 75.0 [-] Show Material materials with Härte, Brinell of 75.0 [-] | T5 | DIN 1725-2, EN 1676, EN 1706 | |
20.0 °C | 80.0 [-] Show Material materials with Härte, Brinell of 80.0 [-] | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 80.0 - 110.0 [-] Show Material materials with Härte, Brinell of 80.0 - 110.0 [-] | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 85.0 - 115.0 [-] Show Material materials with Härte, Brinell of 85.0 - 115.0 [-] | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | |||
Scherfestigkeit | 20.0 °C | 201.0 MPa Show Material materials with Scherfestigkeit of 201.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | |
Schubmodule | 2.8 GPa Show Material materials with Schubmodule of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | |||
Zugfestigkeit | -196.0 °C | 277.0 MPa Show Material materials with Zugfestigkeit of 277.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | |
-196.0 °C | 304.0 MPa Show Material materials with Zugfestigkeit of 304.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
-120.0 °C | 256.0 MPa Show Material materials with Zugfestigkeit of 256.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
-120.0 °C | 275.0 MPa Show Material materials with Zugfestigkeit of 275.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
-50.0 °C | 246.0 MPa Show Material materials with Zugfestigkeit of 246.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
-50.0 °C | 263.0 MPa Show Material materials with Zugfestigkeit of 263.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 200.0 MPa Show Material materials with Zugfestigkeit of 200.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 220.0 MPa Show Material materials with Zugfestigkeit of 220.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 220.0 - 320.0 MPa Show Material materials with Zugfestigkeit of 220.0 - 320.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 235.0 - 251.0 MPa Show Material materials with Zugfestigkeit of 235.0 - 251.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 235.0 MPa Show Material materials with Zugfestigkeit of 235.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 240.0 - 320.0 MPa Show Material materials with Zugfestigkeit of 240.0 - 320.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 241.0 MPa Show Material materials with Zugfestigkeit of 241.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 241.0 - 304.0 MPa Show Material materials with Zugfestigkeit of 241.0 - 304.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 251.0 MPa Show Material materials with Zugfestigkeit of 251.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 304.0 MPa Show Material materials with Zugfestigkeit of 304.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
220.0 °C | 68.0 MPa Show Material materials with Zugfestigkeit of 68.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
220.0 °C | 75.0 MPa Show Material materials with Zugfestigkeit of 75.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
280.0 °C | 48.0 MPa Show Material materials with Zugfestigkeit of 48.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 200.0 °C | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | T5 | DIN 1725-2, EN 1676, EN 1706 | |
Schmelzpunkt | 505.0 - 770.0 °C Show Material materials with Schmelzpunkt of 505.0 - 770.0 °C | Typical for Cast 3xx.x Series Aluminium | |||
Spezifische Wärmekapazität | 20.0 °C | 910.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 910.0 J/(kg·K) | T5 | DIN 1725-2, EN 1676, EN 1706 | |
Wärmeleitfähigkeit | 20.0 °C | 130.0 - 190.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 190.0 W/(m·K) | T5 | DIN 1725-2, EN 1676, EN 1706 |
Elektrisch
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 17000000.0 - 26000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 17000000.0 - 26000000.0 S/m | T5 | DIN 1725-2, EN 1676, EN 1706 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminium | 87.2 % Show Material materials with Aluminium of 87.2 % | T5 | DIN 1725-2, EN 1676, EN 1706 |
Eisen | 0.5 Show Material materials with Eisen of 0.5 | T5 | DIN 1725-2, EN 1676, EN 1706 |
Kupfer | 0.05 Show Material materials with Kupfer of 0.05 | T5 | DIN 1725-2, EN 1676, EN 1706 |
Magnesium | 0.2 - 0.5 % Show Material materials with Magnesium of 0.2 - 0.5 % | T5 | DIN 1725-2, EN 1676, EN 1706 |
Mangan | 0.001 - 0.4 % Show Material materials with Mangan of 0.001 - 0.4 % | T5 | DIN 1725-2, EN 1676, EN 1706 |
Silizium | 9.0 - 11.0 % Show Material materials with Silizium of 9.0 - 11.0 % | T5 | DIN 1725-2, EN 1676, EN 1706 |
Titan | 0.15 Show Material materials with Titan of 0.15 | T5 | DIN 1725-2, EN 1676, EN 1706 |
Zink | 0.1 Show Material materials with Zink of 0.1 | T5 | DIN 1725-2, EN 1676, EN 1706 |
Technological properties
Property | ||
---|---|---|
Processing methods | permanent mould casting |