Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | |
2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | H14 | EN 573-3 | Rod, Flat, Foil, Tube | |
20.0 °C | 2.71 - 2.72 g/cm³ Show Material materials with Dichte of 2.71 - 2.72 g/cm³ | H14 | EN 573-3 | Rod, Flat, Foil, Tube | |
20.0 °C | 2.72 g/cm³ Show Material materials with Dichte of 2.72 g/cm³ | H14 | EN 573-3 | Rod, Flat, Foil, Tube |
Abmessung
Property | Value | Condition | Related Standards | Thickness | Shape |
---|---|---|---|---|---|
Dicke | 60 mm Show Material materials with Dicke of 60 mm | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | 60 mm | Coil, Sheet, Foil |
400 mm Show Material materials with Dicke of 400 mm | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | 400 mm | Coil, Sheet, Foil |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 50.0 MPa Show Material materials with Bending Fatigue Strength of 50.0 MPa | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
Biegewinkel 180° | 1.0 °/t Show Material materials with Biegewinkel 180° of 1.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
1.5 °/t Show Material materials with Biegewinkel 180° of 1.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
Biegewinkel 90° | 0.5 °/t Show Material materials with Biegewinkel 90° of 0.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
1.5 °/t Show Material materials with Biegewinkel 90° of 1.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
2.5 °/t Show Material materials with Biegewinkel 90° of 2.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
Dehnung | 1.0 % Show Material materials with Dehnung of 1.0 % | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | |
1 % Show Material materials with Dehnung of 1 % | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | A50 | ||
2.0 % Show Material materials with Dehnung of 2.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
3.0 % Show Material materials with Dehnung of 3.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
4.0 % Show Material materials with Dehnung of 4.0 % | H14 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A100 | ||
6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A100 | ||
20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | H14 | EN 573-3 | Foil, Flat | A50 | |
20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | H14 | EN 573-3 | Foil | A100 | |
20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H14 | EN 573-3 | Rod, Tube, Flat | A50 | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Rod, Tube | ||
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3 | Flat | ||
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3 | Flat | Transverse | |
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | |||
20.0 °C | 60.0 - 65.0 GPa Show Material materials with Elastizitätsmodul of 60.0 - 65.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
20.0 °C | 60.0 - 69.0 GPa Show Material materials with Elastizitätsmodul of 60.0 - 69.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
20.0 °C | 65.0 - 69.0 GPa Show Material materials with Elastizitätsmodul of 65.0 - 69.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
20.0 °C | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
Härte, Brinell | 37.0 [-] Show Material materials with Härte, Brinell of 37.0 [-] | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 30.0 [-] Show Material materials with Härte, Brinell of 30.0 [-] | H14 | EN 573-3 | Rod, Tube | ||
20.0 °C | 37.0 [-] Show Material materials with Härte, Brinell of 37.0 [-] | H14 | EN 573-3 | Rod, Flat, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | H14 | EN 573-3 | Rod, Flat, Foil, Tube | |
Schubmodule | 25.9 GPa Show Material materials with Schubmodule of 25.9 GPa | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
26.5 GPa Show Material materials with Schubmodule of 26.5 GPa | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | |||
20.0 °C | 24.0 - 26.0 GPa Show Material materials with Schubmodule of 24.0 - 26.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
20.0 °C | 24.0 - 25.9 GPa Show Material materials with Schubmodule of 24.0 - 25.9 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
20.0 °C | 25.9 - 26.0 GPa Show Material materials with Schubmodule of 25.9 - 26.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
20.0 °C | 25.9 GPa Show Material materials with Schubmodule of 25.9 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
Streckgrenze | 80.0 MPa Show Material materials with Streckgrenze of 80.0 MPa | H14 | EN 573-3, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | RP02 | |
95.0 MPa Show Material materials with Streckgrenze of 95.0 MPa | H14 | EN 573-3, EN 485, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | RP02 | ||
95.0 - 150.0 MPa Show Material materials with Streckgrenze of 95.0 - 150.0 MPa | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | |||
20.0 °C | 80.0 MPa Show Material materials with Streckgrenze of 80.0 MPa | H14 | EN 573-3 | Rod, Tube | RP02 | |
20.0 °C | 90.0 MPa Show Material materials with Streckgrenze of 90.0 MPa | H14 | EN 573-3 | Flat | RP02 | |
20.0 °C | 90.0 MPa Show Material materials with Streckgrenze of 90.0 MPa | H14 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 95.0 MPa Show Material materials with Streckgrenze of 95.0 MPa | H14 | EN 573-3 | Foil, Flat | RP02 | |
20.0 °C | 95.0 MPa Show Material materials with Streckgrenze of 95.0 MPa | H14 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 100.0 MPa Show Material materials with Streckgrenze of 100.0 MPa | H14 | EN 573-3 | Foil | RP02 | |
Zugfestigkeit | 105.0 - 170.0 MPa Show Material materials with Zugfestigkeit of 105.0 - 170.0 MPa | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | ||
20.0 °C | 105.0 - 155.0 MPa Show Material materials with Zugfestigkeit of 105.0 - 155.0 MPa | H14 | EN 573-3, EN 683 | Foil, Flat, Strip, Sheet, Plate, Bar, Rod, Tube | ||
20.0 °C | 105.0 - 155.0 MPa Show Material materials with Zugfestigkeit of 105.0 - 155.0 MPa | H14 | EN 573-3 | Flat | Transverse | |
20.0 °C | 110.0 - 145.0 MPa Show Material materials with Zugfestigkeit of 110.0 - 145.0 MPa | H14 | EN 573-3, EN 754 | Rod, Tube, Strip, Sheet, Plate, Foil, Bar | ||
20.0 °C | 110.0 - 160.0 MPa Show Material materials with Zugfestigkeit of 110.0 - 160.0 MPa | H14 | EN 573-3 | Foil | ||
20.0 °C | 115.0 - 155.0 MPa Show Material materials with Zugfestigkeit of 115.0 - 155.0 MPa | H14 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 115.0 - 155.0 MPa Show Material materials with Zugfestigkeit of 115.0 - 155.0 MPa | H14 | EN 573-3 | Flat | Transverse |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.17e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | |
-50.0 °C | 2.17e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
20 °C | 2.17e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
20 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
20 °C | 2.4399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4399999999999997e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20 °C | 2.5399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5399999999999997e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
100 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
100.0 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
100 °C | 0.000024 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.000024 1/K | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | 20-100°C | |
200 °C | 2.4399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4399999999999997e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
200.0 °C | 2.44e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.44e-05 1/K | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
300 °C | 2.5399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5399999999999997e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
300.0 °C | 2.54e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.54e-05 1/K | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
Schmelzpunkt | 644.0 - 657.0 °C Show Material materials with Schmelzpunkt of 644.0 - 657.0 °C | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
Spezifische Wärmekapazität | 20.0 °C | 898.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 898.0 J/(kg·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube | |
Wärmeleitfähigkeit | 138 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 138 W/(m·K) | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | ||
20.0 °C | 205.0 - 210.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 205.0 - 210.0 W/(m·K) | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
20.0 °C | 205.0 - 225.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 205.0 - 225.0 W/(m·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
20.0 °C | 210.0 - 225.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 210.0 - 225.0 W/(m·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
20.0 °C | 225.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 225.0 W/(m·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 33000000.0 - 34000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 33000000.0 - 34000000.0 S/m | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 34400000.0 - 35500000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 34400000.0 - 35500000.0 S/m | H14 | EN 573-3 | Rod, Flat, Foil, Tube | |
spezifischer Widerstand | 2.94e-08 - 3.03e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.94e-08 - 3.03e-08 Ω·m | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
4.9e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.9e-08 Ω·m | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | ||
20.0 °C | 2.95e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.95e-08 Ω·m | H14 | EN 573-3 | Rod, Flat, Foil, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Aluminium | 99.0 % Show Material materials with Aluminium of 99.0 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Bar | |
Andere | 0.15 % Show Material materials with Andere of 0.15 % | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | |
Eisen | 1 % Show Material materials with Eisen of 1 % | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | Si + Fe |
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Bar | |
0.05 % Show Material materials with Kupfer of 0.05 % | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | ||
Mangan | 0.05 % Show Material materials with Mangan of 0.05 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Bar | |
0.05 % Show Material materials with Mangan of 0.05 % | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | ||
Silizium | 1 % Show Material materials with Silizium of 1 % | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | Si + Fe |
Titan | 0.05 % Show Material materials with Titan of 0.05 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Bar | |
0.05 % Show Material materials with Titan of 0.05 % | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil | ||
Zink | 0.1 % Show Material materials with Zink of 0.1 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Bar | |
0.1 % Show Material materials with Zink of 0.1 % | H14 | EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 485-2 | Coil, Sheet, Foil |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels; Roofing: Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels; Electronic devices: Housing of devices; Heat exchangers: Fins; Cable wrapping: Electric cable wrapping; Insulation; Solar: Solar collectors; Semi-rigid and corrugated: Smooth wall | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: sufficient, weathering: acceptable | |
Welding | Excellent | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H12) / very good (H12) |