Allgemein
Property | Temperature | Value | Comment |
---|---|---|---|
Dichte | 23.0 °C | 10.5 g/cm³ Show Material materials with Dichte of 10.5 g/cm³ | Typical for Silver |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 43 % Show Material materials with Dehnung of 43 % | |
200.0 °C | 41 % Show Material materials with Dehnung of 41 % | ||
400.0 °C | 38 % Show Material materials with Dehnung of 38 % | ||
600.0 °C | 41 % Show Material materials with Dehnung of 41 % | ||
800.0 °C | 62 % Show Material materials with Dehnung of 62 % | ||
Elastizitätsmodul | 23.0 °C | 83 GPa Show Material materials with Elastizitätsmodul of 83 GPa | Typical for Silver |
Poissonzahl | 23.0 °C | 0.37 [-] Show Material materials with Poissonzahl of 0.37 [-] | Typical for Silver |
Schubmodule | 23.0 °C | 30 GPa Show Material materials with Schubmodule of 30 GPa | Typical for Silver |
Zugfestigkeit | 20.0 °C | 240 MPa Show Material materials with Zugfestigkeit of 240 MPa | |
200.0 °C | 200 MPa Show Material materials with Zugfestigkeit of 200 MPa | ||
400.0 °C | 170 MPa Show Material materials with Zugfestigkeit of 170 MPa | ||
600.0 °C | 100 MPa Show Material materials with Zugfestigkeit of 100 MPa | ||
800.0 °C | 40 MPa Show Material materials with Zugfestigkeit of 40 MPa | ||
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 23.0 °C | 1.9E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.9E-5 1/K | Typical for Silver |
Schmelzpunkt | 962 °C Show Material materials with Schmelzpunkt of 962 °C | Typical for Silver | |
Spezifische Wärmekapazität | 23.0 °C | 234 - 251 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 234 - 251 J/(kg·K) | Typical for Silver |
Wärmeleitfähigkeit | 23.0 °C | 417 - 428 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 417 - 428 W/(m·K) | Typical for Silver |