Property | Temperature | Value |
---|---|---|
Dichte | 20.0 °C | 18.7 g/cm³ Show Material materials with Dichte of 18.7 g/cm³ |
Mechanisch
Property | Temperature | Value | Comment |
---|---|---|---|
Dehnung | 20.0 °C | 2 % Show Material materials with Dehnung of 2 % | |
Elastizitätsmodul | 20.0 °C | 240 GPa Show Material materials with Elastizitätsmodul of 240 GPa | |
Härte, Vickers | 20.0 °C | 273 [-] Show Material materials with Härte, Vickers of 273 [-] | |
Poissonzahl | 23.0 °C | 0.39 [-] Show Material materials with Poissonzahl of 0.39 [-] | Typical for Platinum |
Schubmodule | 20.0 °C | 86 GPa Show Material materials with Schubmodule of 86 GPa | |
Streckgrenze Rp 0,2 | 20.0 °C | 920 MPa Show Material materials with Streckgrenze Rp 0,2 of 920 MPa | |
Zugfestigkeit | 20.0 °C | 940 MPa Show Material materials with Zugfestigkeit of 940 MPa |
Thermisch
Property | Temperature | Value | Comment |
---|---|---|---|
Koeffizient der thermischen Ausdehnung | 300.0 °C | 1.04E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.04E-5 1/K | |
700.0 °C | 1.09E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.09E-5 1/K | ||
1200.0 °C | 1.15E-5 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.15E-5 1/K | ||
Schmelzpunkt | 1769 °C Show Material materials with Schmelzpunkt of 1769 °C | Typical for Platinum | |
Spezifische Wärmekapazität | 23.0 °C | 136 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 136 J/(kg·K) | Typical for Platinum |
Wärmeleitfähigkeit | 20.0 °C | 28 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 28 W/(m·K) |
Elektrisch
Property | Temperature | Value |
---|---|---|
spezifischer Widerstand | 20.0 °C | 2.14E-7 Ω·m Show Material materials with spezifischer Widerstand of 2.14E-7 Ω·m |