Allgemein
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Dichte | 20.0 °C | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | T5 | WL 3.2364 |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Dehnung | 20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | T5 | WL 3.2364 | |
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | T5 | WL 3.2364 | ||
24.0 °C | 3.5 % Show Material materials with Dehnung of 3.5 % | T5 | WL 3.2364 | A50 | |
24.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | T5 | WL 3.2364 | A50 | |
100.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | T5 | WL 3.2364 | A50 | |
100.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | T5 | WL 3.2364 | A50 | |
149.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | T5 | WL 3.2364 | A50 | |
149.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | T5 | WL 3.2364 | A50 | |
204.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | T5 | WL 3.2364 | A50 | |
204.0 °C | 30.0 % Show Material materials with Dehnung of 30.0 % | T5 | WL 3.2364 | A50 | |
260.0 °C | 30.0 % Show Material materials with Dehnung of 30.0 % | T5 | WL 3.2364 | A50 | |
260.0 °C | 55.0 % Show Material materials with Dehnung of 55.0 % | T5 | WL 3.2364 | A50 | |
316.0 °C | 60.0 % Show Material materials with Dehnung of 60.0 % | T5 | WL 3.2364 | A50 | |
316.0 °C | 70.0 % Show Material materials with Dehnung of 70.0 % | T5 | WL 3.2364 | A50 | |
371.0 °C | 75.0 % Show Material materials with Dehnung of 75.0 % | T5 | WL 3.2364 | A50 | |
371.0 °C | 80.0 % Show Material materials with Dehnung of 80.0 % | T5 | WL 3.2364 | A50 | |
Elastizitätsmodul | 20.0 °C | 70.6 GPa Show Material materials with Elastizitätsmodul of 70.6 GPa | T5 | WL 3.2364 | |
Härte, Brinell | 20.0 °C | 70.0 [-] Show Material materials with Härte, Brinell of 70.0 [-] | T5 | WL 3.2364 | |
20.0 °C | 75.0 [-] Show Material materials with Härte, Brinell of 75.0 [-] | T5 | WL 3.2364 | ||
20.0 °C | 80.0 [-] Show Material materials with Härte, Brinell of 80.0 [-] | T5 | WL 3.2364 | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | |||
Scherfestigkeit | 20.0 °C | 177.0 MPa Show Material materials with Scherfestigkeit of 177.0 MPa | T5 | WL 3.2364 | |
Schubmodule | 2.8 GPa Show Material materials with Schubmodule of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | |||
Zugfestigkeit | 20.0 °C | 167.0 MPa Show Material materials with Zugfestigkeit of 167.0 MPa | T5 | WL 3.2364 | |
20.0 °C | 177.0 MPa Show Material materials with Zugfestigkeit of 177.0 MPa | T5 | WL 3.2364 | ||
20.0 °C | 216.0 MPa Show Material materials with Zugfestigkeit of 216.0 MPa | T5 | WL 3.2364 | ||
20.0 °C | 235.0 MPa Show Material materials with Zugfestigkeit of 235.0 MPa | T5 | WL 3.2364 | ||
24.0 °C | 226.0 MPa Show Material materials with Zugfestigkeit of 226.0 MPa | T5 | WL 3.2364 | ||
24.0 °C | 265.0 MPa Show Material materials with Zugfestigkeit of 265.0 MPa | T5 | WL 3.2364 | ||
100.0 °C | 206.0 MPa Show Material materials with Zugfestigkeit of 206.0 MPa | T5 | WL 3.2364 | ||
149.0 °C | 147.0 MPa Show Material materials with Zugfestigkeit of 147.0 MPa | T5 | WL 3.2364 | ||
149.0 °C | 157.0 MPa Show Material materials with Zugfestigkeit of 157.0 MPa | T5 | WL 3.2364 | ||
204.0 °C | 82.0 MPa Show Material materials with Zugfestigkeit of 82.0 MPa | T5 | WL 3.2364 | ||
260.0 °C | 52.0 MPa Show Material materials with Zugfestigkeit of 52.0 MPa | T5 | WL 3.2364 | ||
316.0 °C | 27.0 MPa Show Material materials with Zugfestigkeit of 27.0 MPa | T5 | WL 3.2364 | ||
371.0 °C | 18.0 MPa Show Material materials with Zugfestigkeit of 18.0 MPa | T5 | WL 3.2364 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50.0 °C | 2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2e-05 1/K | T5 | WL 3.2364 | |
100.0 °C | 2.14e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.14e-05 1/K | T5 | WL 3.2364 | ||
200.0 °C | 2.25e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.25e-05 1/K | T5 | WL 3.2364 | ||
300.0 °C | 2.33e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.33e-05 1/K | T5 | WL 3.2364 | ||
Schmelzpunkt | 505.0 - 770.0 °C Show Material materials with Schmelzpunkt of 505.0 - 770.0 °C | Typical for Cast 3xx.x Series Aluminium | |||
Spezifische Wärmekapazität | 960.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 960.0 - 963.0 J/(kg·K) | Typical for Cast 3xx.x Series Aluminium | |||
Wärmeleitfähigkeit | 130.0 - 180.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 180.0 W/(m·K) | Typical for Cast 3xx.x Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Eisen | 0.6 Show Material materials with Eisen of 0.6 | T5 | WL 3.2364 |
Kupfer | 0.2 Show Material materials with Kupfer of 0.2 | T5 | WL 3.2364 |
Magnesium | 0.2 - 0.4 % Show Material materials with Magnesium of 0.2 - 0.4 % | T5 | WL 3.2364 |
Mangan | 0.35 Show Material materials with Mangan of 0.35 | T5 | WL 3.2364 |
Silizium | 6.5 - 7.5 % Show Material materials with Silizium of 6.5 - 7.5 % | T5 | WL 3.2364 |
Titan | 0.25 Show Material materials with Titan of 0.25 | T5 | WL 3.2364 |
Zink | 0.3 Show Material materials with Zink of 0.3 | T5 | WL 3.2364 |
Technological properties
Property | ||
---|---|---|
Processing methods | permanent mould casting, sample taken from casting |